General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.82 g/cm³ Show Material materials with Densidad of 2.82 g/cm³ | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
2.83 g/cm³ Show Material materials with Densidad of 2.83 g/cm³ | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 2.82 g/cm³ Show Material materials with Densidad of 2.82 g/cm³ | T6 | EN 573-3 | Rod, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 110.0 [-] Show Material materials with Dureza Brinell of 110.0 [-] | T6 | EN 573-3 | Rod, Tube | |
Elongación | 4.0 % Show Material materials with Elongación of 4.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A50 | |
6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
8.0 % Show Material materials with Elongación of 8.0 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T6 | EN 573-3 | Tube | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3 | Rod | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3 | Tube, Rod | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T6 | EN 573-3 | Rod | ||
Módulo de cizallamiento | 27.3 GPa Show Material materials with Módulo de cizallamiento of 27.3 GPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
72.5 GPa Show Material materials with Módulo elástico of 72.5 GPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Resistencia a la tracción | 295.0 MPa Show Material materials with Resistencia a la tracción of 295.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |||
20.0 °C | 295.0 MPa Show Material materials with Resistencia a la tracción of 295.0 MPa | T6 | EN 573-3 | Rod | ||
20.0 °C | 310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T6 | EN 573-3 | Tube, Rod |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 864.0 J/(kg·K) Show Material materials with Calor específico of 864.0 J/(kg·K) | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 864.0 J/(kg·K) Show Material materials with Calor específico of 864.0 J/(kg·K) | T6 | EN 573-3 | Rod, Tube | |
Coeficiente de dilatación térmica | -50 °C | 2.14e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.14e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar, Rod |
-50.0 °C | 2.14e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.14e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar, Rod | |
20 °C | 2.14e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.14e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar, Rod | |
20 °C | 2.2899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2899999999999998e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar, Rod | |
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4999999999999998e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2899999999999998e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
100.0 °C | 2.29e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.29e-05 1/K | T6 | EN 573-3 | Rod, Tube | |
100.0 °C | 2.29e-05 - 2.31e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.29e-05 - 2.31e-05 1/K | T6 | EN 573-3 | Rod, Tube | |
100.0 °C | 2.31e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.31e-05 1/K | T6 | EN 573-3 | Rod, Tube | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
200 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar, Rod | |
200.0 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar, Rod | |
300 °C | 2.4999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4999999999999998e-05 1/K | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
300.0 °C | 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5e-05 1/K | T6 | EN 573-3 | Rod, Tube | |
Conductividad térmica | 170.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 220.0 W/(m·K) | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 151.0 - 172.0 W/(m·K) Show Material materials with Conductividad térmica of 151.0 - 172.0 W/(m·K) | T6 | EN 573-3, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar | |
Temperatura de fusión | 540.0 - 645.0 °C Show Material materials with Temperatura de fusión of 540.0 - 645.0 °C | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
585.0 - 650.0 °C Show Material materials with Temperatura de fusión of 585.0 - 650.0 °C | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 24000000.0 - 32000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 32000000.0 S/m | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 23000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 26000000.0 S/m | T6 | EN 573-3, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar | |
Resistividad eléctrica | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.13e-08 - 4.17e-08 Ω·m | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 - 4.35e-08 Ω·m | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bismuto | 0.2 - 0.6 % Show Material materials with Bismuto of 0.2 - 0.6 % | T6 | EN 573-3, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
Cobre | 4.5 - 6.0 % Show Material materials with Cobre of 4.5 - 6.0 % | T6 | EN 573-3 | Rod, Tube |
5.0 - 6.0 % Show Material materials with Cobre of 5.0 - 6.0 % | T6 | EN 573-3, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar | |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T6 | EN 573-3 | Rod, Tube |
0.7 % Show Material materials with Hierro of 0.7 % | T6 | EN 573-3 | Rod, Tube | |
0.70 % Show Material materials with Hierro of 0.70 % | T6 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Plomo | 0.2 - 0.6 % Show Material materials with Plomo of 0.2 - 0.6 % | T6 | EN 573-3, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | T6 | EN 573-3, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
Zinc | 0.3 % Show Material materials with Zinc of 0.3 % | T6 | EN 573-3, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: poor | |
Brazing | hard brazing (with flux/ without flux): not suitable /, friction soldering: sufficient | |
Corrosion properties | Seawater: poor, weathering: sufficient | |
Workability | Deep drawing / upsetting (Condition) - / acceptable |