General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T3 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 140.0 MPa Show Material materials with Bending Fatigue Strength of 140.0 MPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 123.0 [-] Show Material materials with Dureza Brinell of 123.0 [-] | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
124.0 [-] Show Material materials with Dureza Brinell of 124.0 [-] | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
20.0 °C | 104.0 - 120.0 [-] Show Material materials with Dureza Brinell of 104.0 - 120.0 [-] | T3 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 104.0 - 115.0 [-] Show Material materials with Dureza Brinell of 104.0 - 115.0 [-] | T3 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 104.0 - 110.0 [-] Show Material materials with Dureza Brinell of 104.0 - 110.0 [-] | T3 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 104.0 [-] Show Material materials with Dureza Brinell of 104.0 [-] | T3 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 104.0 - 123.0 [-] Show Material materials with Dureza Brinell of 104.0 - 123.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 104.0 - 124.0 [-] Show Material materials with Dureza Brinell of 104.0 - 124.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 104.0 - 122.0 [-] Show Material materials with Dureza Brinell of 104.0 - 122.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 110.0 [-] Show Material materials with Dureza Brinell of 110.0 [-] | T3 | EN 573-3 | Profile, Sheet, Flat | ||
20.0 °C | 110.0 - 138.0 [-] Show Material materials with Dureza Brinell of 110.0 - 138.0 [-] | T3 | EN 573-3 | Profile | ||
20.0 °C | 110.0 - 120.0 [-] Show Material materials with Dureza Brinell of 110.0 - 120.0 [-] | T3 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 110.0 - 115.0 [-] Show Material materials with Dureza Brinell of 110.0 - 115.0 [-] | T3 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 110.0 - 123.0 [-] Show Material materials with Dureza Brinell of 110.0 - 123.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 110.0 - 124.0 [-] Show Material materials with Dureza Brinell of 110.0 - 124.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 110.0 - 122.0 [-] Show Material materials with Dureza Brinell of 110.0 - 122.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 115.0 [-] Show Material materials with Dureza Brinell of 115.0 [-] | T3 | EN 573-3 | Tube, Sheet, Flat | ||
20.0 °C | 115.0 - 120.0 [-] Show Material materials with Dureza Brinell of 115.0 - 120.0 [-] | T3 | EN 573-3 | Tube, Sheet, Flat | ||
20.0 °C | 115.0 - 123.0 [-] Show Material materials with Dureza Brinell of 115.0 - 123.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 115.0 - 124.0 [-] Show Material materials with Dureza Brinell of 115.0 - 124.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 115.0 - 122.0 [-] Show Material materials with Dureza Brinell of 115.0 - 122.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 120.0 [-] Show Material materials with Dureza Brinell of 120.0 [-] | T3 | EN 573-3 | Profile, Rod, Tube, Sheet, Flat | ||
20.0 °C | 120.0 - 123.0 [-] Show Material materials with Dureza Brinell of 120.0 - 123.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 120.0 - 124.0 [-] Show Material materials with Dureza Brinell of 120.0 - 124.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 120.0 - 122.0 [-] Show Material materials with Dureza Brinell of 120.0 - 122.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 122.0 - 124.0 [-] Show Material materials with Dureza Brinell of 122.0 - 124.0 [-] | T3 | EN 573-3 | Rod, Flat | ||
20.0 °C | 122.0 [-] Show Material materials with Dureza Brinell of 122.0 [-] | T3 | EN 573-3 | Rod, Flat | ||
20.0 °C | 122.0 - 123.0 [-] Show Material materials with Dureza Brinell of 122.0 - 123.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 123.0 [-] Show Material materials with Dureza Brinell of 123.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 123.0 - 124.0 [-] Show Material materials with Dureza Brinell of 123.0 - 124.0 [-] | T3 | EN 573-3 | Flat | ||
20.0 °C | 124.0 [-] Show Material materials with Dureza Brinell of 124.0 [-] | T3 | EN 573-3 | Rod, Flat | ||
20.0 °C | 137.0 [-] Show Material materials with Dureza Brinell of 137.0 [-] | T3 | EN 573-3 | Tube | ||
20.0 °C | 138.0 [-] Show Material materials with Dureza Brinell of 138.0 [-] | T3 | EN 573-3 | Profile | ||
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T3 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | |
7.0 % Show Material materials with Elongación of 7.0 % | T3 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A100 | ||
9.0 % Show Material materials with Elongación of 9.0 % | T3 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A100 | ||
10.0 % Show Material materials with Elongación of 10.0 % | T3 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A100 | ||
12.0 % Show Material materials with Elongación of 12.0 % | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | ||
13.0 % Show Material materials with Elongación of 13.0 % | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T3 | EN 573-3 | Sheet | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T3 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T3 | EN 573-3 | Sheet | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T3 | EN 573-3 | Rod | A50 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3 | Tube, Sheet, Profile, Rod | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T3 | EN 573-3 | Rod | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T3 | EN 573-3 | Rod, Tube | ||
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | T3 | EN 573-3 | Flat | ||
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | T3 | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | T3 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T3 | EN 573-3 | Flat | A50 | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T3 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T3 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T3 | EN 573-3 | Flat | A50 Transverse | |
Límite elástico | 270.0 MPa Show Material materials with Límite elástico of 270.0 MPa | T3 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | RP02 | |
280.0 MPa Show Material materials with Límite elástico of 280.0 MPa | T3 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | RP02 | ||
290.0 MPa Show Material materials with Límite elástico of 290.0 MPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | RP02 | ||
300.0 MPa Show Material materials with Límite elástico of 300.0 MPa | T3 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | RP02 | ||
310.0 MPa Show Material materials with Límite elástico of 310.0 MPa | T3 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | RP02 | ||
20.0 °C | 140.0 MPa Show Material materials with Límite elástico of 140.0 MPa | T3 | EN 573-3 | RP02 Transverse | ||
20.0 °C | 250.0 MPa Show Material materials with Límite elástico of 250.0 MPa | T3 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 250.0 MPa Show Material materials with Límite elástico of 250.0 MPa | T3 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 270.0 MPa Show Material materials with Límite elástico of 270.0 MPa | T3 | EN 573-3 | Tube, Sheet, Rod | RP02 | |
20.0 °C | 270.0 MPa Show Material materials with Límite elástico of 270.0 MPa | T3 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 275.0 - 310.0 MPa Show Material materials with Límite elástico of 275.0 - 310.0 MPa | T3 | EN 573-3 | |||
20.0 °C | 280.0 MPa Show Material materials with Límite elástico of 280.0 MPa | T3 | EN 573-3 | Rod | RP02 | |
20.0 °C | 285.0 MPa Show Material materials with Límite elástico of 285.0 MPa | T3 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 285.0 MPa Show Material materials with Límite elástico of 285.0 MPa | T3 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 290.0 MPa Show Material materials with Límite elástico of 290.0 MPa | T3 | EN 573-3 | Tube, Sheet, Flat, Profile, Rod | RP02 | |
20.0 °C | 290.0 MPa Show Material materials with Límite elástico of 290.0 MPa | T3 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 300.0 MPa Show Material materials with Límite elástico of 300.0 MPa | T3 | EN 573-3 | Rod | RP02 | |
20.0 °C | 310.0 MPa Show Material materials with Límite elástico of 310.0 MPa | T3 | EN 573-3 | Rod | RP02 | |
20.0 °C | 450.0 MPa Show Material materials with Límite elástico of 450.0 MPa | T3 | EN 573-3 | Flat | Transverse | |
Módulo de cizallamiento | 27.4 GPa Show Material materials with Módulo de cizallamiento of 27.4 GPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 27.0 - 28.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 - 28.0 GPa | T3 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 70.0 - 74.5 GPa Show Material materials with Módulo elástico of 70.0 - 74.5 GPa | T3 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Plane-Strain Fracture Toughnes | 20.0 °C | 17.5 - 41.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 17.5 - 41.7 MPa·√m | T3 | EN 573-3 | ||
20.0 °C | 17.5 - 33.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 17.5 - 33.5 MPa·√m | T3 | EN 573-3 | |||
20.0 °C | 17.5 - 18.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 17.5 - 18.0 MPa·√m | T3 | EN 573-3 | |||
20.0 °C | 18.0 - 41.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 41.7 MPa·√m | T3 | EN 573-3 | |||
20.0 °C | 18.0 - 33.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 33.5 MPa·√m | T3 | EN 573-3 | |||
20.0 °C | 18.0 - 26.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 26.2 MPa·√m | T3 | EN 573-3 | |||
20.0 °C | 18.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.0 MPa·√m | T3 | EN 573-3 | |||
20.0 °C | 26.2 - 41.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 41.7 MPa·√m | T3 | EN 573-3 | |||
20.0 °C | 26.2 - 33.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 33.5 MPa·√m | T3 | EN 573-3 | |||
Resistencia a la tracción | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T3 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T3 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T3 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
425.0 MPa Show Material materials with Resistencia a la tracción of 425.0 MPa | T3 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T3 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
20.0 °C | 220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | T3 | EN 573-3 | Transverse | ||
20.0 °C | 360.0 MPa Show Material materials with Resistencia a la tracción of 360.0 MPa | T3 | EN 573-3 | Sheet | ||
20.0 °C | 360.0 MPa Show Material materials with Resistencia a la tracción of 360.0 MPa | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 380.0 MPa Show Material materials with Resistencia a la tracción of 380.0 MPa | T3 | EN 573-3 | Sheet | ||
20.0 °C | 380.0 MPa Show Material materials with Resistencia a la tracción of 380.0 MPa | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T3 | EN 573-3 | Profile | ||
20.0 °C | 400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T3 | EN 573-3 | Sheet, Rod | ||
20.0 °C | 400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T3 | EN 573-3 | Tube, Sheet, Profile, Rod | ||
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 425.0 MPa Show Material materials with Resistencia a la tracción of 425.0 MPa | T3 | EN 573-3 | Rod | ||
20.0 °C | 430.0 MPa Show Material materials with Resistencia a la tracción of 430.0 MPa | T3 | EN 573-3 | Flat | ||
20.0 °C | 430.0 MPa Show Material materials with Resistencia a la tracción of 430.0 MPa | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T3 | EN 573-3 | Flat | ||
20.0 °C | 435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T3 | EN 573-3 | Tube, Flat, Rod | ||
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T3 | EN 573-3 | Flat | Transverse | |
20.0 °C | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T3 | EN 573-3 | Rod | ||
Ángulo de flexión a 180° | 4.0 °/t Show Material materials with Ángulo de flexión a 180° of 4.0 °/t | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
5.0 °/t Show Material materials with Ángulo de flexión a 180° of 5.0 °/t | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
Ángulo de flexión a 90° | 4.0 °/t Show Material materials with Ángulo de flexión a 90° of 4.0 °/t | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
5.0 °/t Show Material materials with Ángulo de flexión a 90° of 5.0 °/t | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
8.0 °/t Show Material materials with Ángulo de flexión a 90° of 8.0 °/t | T3 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | T3 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
Coeficiente de dilatación térmica | -50 °C | 2.11e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.11e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
20 °C | 2.11e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.11e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.2899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2899999999999998e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2899999999999998e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
200 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
300 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Conductividad térmica | 121.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 121.0 - 193.0 W/(m·K) | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | T3 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar | |
Temperatura de fusión | 505.0 - 640.0 °C Show Material materials with Temperatura de fusión of 505.0 - 640.0 °C | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
505.0 - 635.0 °C Show Material materials with Temperatura de fusión of 505.0 - 635.0 °C | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 17000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 29000000.0 S/m | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 18000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 21000000.0 S/m | T3 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar | |
Resistividad eléctrica | 3.45e-08 - 5.88e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 5.88e-08 Ω·m | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
4.76e-08 - 5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.56e-08 Ω·m | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 3.8 - 4.9 % Show Material materials with Cobre of 3.8 - 4.9 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T3 | EN 573-3 | Sheet, Flat, Profile, Rod, Tube |
0.50 % Show Material materials with Hierro of 0.50 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Magnesio | 1.2 - 1.8 % Show Material materials with Magnesio of 1.2 - 1.8 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Manganeso | 0.3 - 0.9 % Show Material materials with Manganeso of 0.3 - 0.9 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: poor, weathering: poor | |
Workability | Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O) |