General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Coil, Sheet, Foil |
Medidas
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Espesor | 0.2 mm Show Material materials with Espesor of 0.2 mm | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | 0.2 mm | Coil, Sheet, Foil |
2.0 mm Show Material materials with Espesor of 2.0 mm | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | 2.0 mm | Coil, Sheet, Foil |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 50.0 MPa Show Material materials with Bending Fatigue Strength of 50.0 MPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | |
Dureza Brinell | 28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | O | EN 573-3 | Flat, Sheet | ||
20.0 °C | 29.0 [-] Show Material materials with Dureza Brinell of 29.0 [-] | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 30.0 [-] Show Material materials with Dureza Brinell of 30.0 [-] | O | EN 573-3 | Rod, Tube | ||
Dureza Brinell (HBW) | 25.0 - 60.0 [-] Show Material materials with Dureza Brinell (HBW) of 25.0 - 60.0 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | ||
Elongación | -196.0 °C | 46.0 % Show Material materials with Elongación of 46.0 % | O | EN 573-3 | ||
-80.0 °C | 42.0 % Show Material materials with Elongación of 42.0 % | O | EN 573-3 | |||
-28.0 °C | 41.0 % Show Material materials with Elongación of 41.0 % | O | EN 573-3 | |||
1 % Show Material materials with Elongación of 1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | A50 | ||
7.0 % Show Material materials with Elongación of 7.0 % | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
21.0 % Show Material materials with Elongación of 21.0 % | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
25.0 % Show Material materials with Elongación of 25.0 % | O | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Rod | A50 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Sheet | A50 | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 21.0 % Show Material materials with Elongación of 21.0 % | O | EN 573-3 | Profile, Rod | ||
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3 | Sheet | ||
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3 | Sheet, Flat | A50 | |
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3 | Wire | A100 | |
20.0 °C | 40.0 % Show Material materials with Elongación of 40.0 % | O | EN 573-3 | |||
100.0 °C | 43.0 % Show Material materials with Elongación of 43.0 % | O | EN 573-3 | |||
150.0 °C | 47.0 % Show Material materials with Elongación of 47.0 % | O | EN 573-3 | |||
200.0 °C | 60.0 % Show Material materials with Elongación of 60.0 % | O | EN 573-3 | |||
260.0 °C | 65.0 % Show Material materials with Elongación of 65.0 % | O | EN 573-3 | |||
315.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | O | EN 573-3 | |||
370.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | O | EN 573-3 | |||
Límite elástico | -270 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat | RP02 |
-270.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat | RP02 | |
-196.0 °C | 60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3 | Wire | RP02 | |
-80.0 °C | 50.0 MPa Show Material materials with Límite elástico of 50.0 MPa | O | EN 573-3 | RP02 | ||
-28.0 °C | 45.0 MPa Show Material materials with Límite elástico of 45.0 MPa | O | EN 573-3 | RP02 | ||
35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
35 MPa Show Material materials with Límite elástico of 35 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |||
60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
20.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat | RP02 | |
20 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat | RP02 | |
20.0 °C | 35.0 - 40.0 MPa Show Material materials with Límite elástico of 35.0 - 40.0 MPa | O | EN 573-3 | RP02 | ||
20.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | EN 573-3 | RP02 | ||
20.0 °C | 60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3 | Wire | RP02 | |
20.0 °C | 65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | O | EN 573-3 | Foil | RP02 | |
20.0 °C | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | O | EN 573-3 | Foil | RP02 | |
50 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat | RP02 | |
50.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat | RP02 | |
100.0 °C | 40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | EN 573-3 | RP02 | ||
150.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat | RP02 | |
200.0 °C | 30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | O | EN 573-3 | RP02 | ||
260.0 °C | 25.0 MPa Show Material materials with Límite elástico of 25.0 MPa | O | EN 573-3 | RP02 | ||
315.0 °C | 15.0 MPa Show Material materials with Límite elástico of 15.0 MPa | O | EN 573-3 | RP02 | ||
370.0 °C | 10.0 MPa Show Material materials with Límite elástico of 10.0 MPa | O | EN 573-3 | RP02 | ||
Módulo de cizallamiento | 26.0 GPa Show Material materials with Módulo de cizallamiento of 26.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | ||
26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.1 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.1 - 26.5 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
Módulo elástico | -270 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | |
-270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Módulo elástico of 60.0 - 70.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 60.0 - 69.5 GPa Show Material materials with Módulo elástico of 60.0 - 69.5 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Módulo elástico of 60.0 - 69.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 65.0 - 70.0 GPa Show Material materials with Módulo elástico of 65.0 - 70.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 65.0 - 69.5 GPa Show Material materials with Módulo elástico of 65.0 - 69.5 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Módulo elástico of 65.0 - 69.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat, Coil, Sheet, Foil | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Módulo elástico of 69.0 - 69.5 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Módulo elástico of 69.5 - 70.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat, Coil, Sheet, Foil | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
300 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | -196.0 °C | 230.0 MPa Show Material materials with Resistencia a la tracción of 230.0 MPa | O | EN 573-3 | ||
-80.0 °C | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | O | EN 573-3 | |||
-28.0 °C | 120.0 MPa Show Material materials with Resistencia a la tracción of 120.0 MPa | O | EN 573-3 | |||
95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
95 MPa Show Material materials with Resistencia a la tracción of 95 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |||
100.0 MPa Show Material materials with Resistencia a la tracción of 100.0 MPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 80.0 - 130.0 MPa Show Material materials with Resistencia a la tracción of 80.0 - 130.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 85.0 - 135.0 MPa Show Material materials with Resistencia a la tracción of 85.0 - 135.0 MPa | O | EN 573-3, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | O | EN 573-3 | Profile, Rod | ||
20.0 °C | 95.0 - 130.0 MPa Show Material materials with Resistencia a la tracción of 95.0 - 130.0 MPa | O | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar | ||
20.0 °C | 95.0 - 135.0 MPa Show Material materials with Resistencia a la tracción of 95.0 - 135.0 MPa | O | EN 573-3, EN 485, EN 755 | Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar, Flat | ||
20.0 °C | 95.0 - 135.0 MPa Show Material materials with Resistencia a la tracción of 95.0 - 135.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 100.0 MPa Show Material materials with Resistencia a la tracción of 100.0 MPa | O | EN 573-3 | Sheet | ||
20.0 °C | 110.0 MPa Show Material materials with Resistencia a la tracción of 110.0 MPa | O | EN 573-3 | |||
20.0 °C | 130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | O | EN 573-3 | Wire | ||
100.0 °C | 90.0 MPa Show Material materials with Resistencia a la tracción of 90.0 MPa | O | EN 573-3 | |||
150.0 °C | 75.0 MPa Show Material materials with Resistencia a la tracción of 75.0 MPa | O | EN 573-3 | |||
200.0 °C | 60.0 MPa Show Material materials with Resistencia a la tracción of 60.0 MPa | O | EN 573-3 | |||
260.0 °C | 40.0 MPa Show Material materials with Resistencia a la tracción of 40.0 MPa | O | EN 573-3 | |||
315.0 °C | 30.0 MPa Show Material materials with Resistencia a la tracción of 30.0 MPa | O | EN 573-3 | |||
370.0 °C | 20.0 MPa Show Material materials with Resistencia a la tracción of 20.0 MPa | O | EN 573-3 | |||
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | ||
1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Ángulo de flexión a 90° | 1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Calor específico of 892.0 - 893.0 J/(kg·K) | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 892.0 J/(kg·K) Show Material materials with Calor específico of 892.0 J/(kg·K) | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
Coeficiente de dilatación térmica | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.15e-05 1/K | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
100 °C | 0.000023 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000023 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | 20-100°C | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.32e-05 1/K | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
200 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
200.0 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
300 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
300.0 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
Conductividad térmica | 159.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 159.0 - 193.0 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
176 W/(m·K) Show Material materials with Conductividad térmica of 176 W/(m·K) | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20.0 °C | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | ||
Temperatura de fusión | 640.0 - 655.0 °C Show Material materials with Temperatura de fusión of 640.0 - 655.0 °C | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
643.0 - 654.0 °C Show Material materials with Temperatura de fusión of 643.0 - 654.0 °C | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 24000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 29000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 29000000.0 S/m | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | |
20.0 °C | 23000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 29000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | |
Resistividad eléctrica | 3.4e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |
3.45e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 4.17e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
3.45e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 4.35e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.1e-08 Ω·m | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.5e-08 Ω·m | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 Ω·m | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 - 4.5e-08 Ω·m | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 - 0.2 % Show Material materials with Cobre of 0.05 - 0.2 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar, Coil, Sheet, Foil |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-3 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire |
0.70 % Show Material materials with Hierro of 0.70 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar, Coil, Sheet, Foil |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar |
0.6 % Show Material materials with Silicona of 0.6 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar |
0.1 % Show Material materials with Zinc of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Electronic devices: Housing of devices; Heat exchangers: Fins, Heat exchangers, General appliacations; Tubes: Industrial tubes, Flexible tube, Pipes; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Automotive trim: Interior trims; Components: Heat shields, Automotive fins, Heat exchangers, General transportation | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |