General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | |||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | |||
Resistencia a la tracción | 140.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 140.0 - 200.0 MPa | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Ángulo de flexión a 90° | 1.25 °/t Show Material materials with Ángulo de flexión a 90° of 1.25 °/t | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Coeficiente de dilatación térmica | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
200 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
300 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Conductividad térmica | 159.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 159.0 - 193.0 W/(m·K) | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Temperatura de fusión | 640.0 - 655.0 °C Show Material materials with Temperatura de fusión of 640.0 - 655.0 °C | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
643.0 - 654.0 °C Show Material materials with Temperatura de fusión of 643.0 - 654.0 °C | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 29000000.0 S/m | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
24000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 29000000.0 S/m | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Resistividad eléctrica | 3.45e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 4.17e-08 Ω·m | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
3.45e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 4.35e-08 Ω·m | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 - 0.2 % Show Material materials with Cobre of 0.05 - 0.2 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |