General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H44 | EN 573-3 | Sheet, Strip |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 66.0 [-] Show Material materials with Dureza Brinell of 66.0 [-] | H44 | EN 573-3 | Flat | |
Módulo de cizallamiento | 20.0 °C | 25.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 27.0 GPa | H44 | EN 573-3 | Sheet, Strip | |
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 210.0 - 265.0 MPa Show Material materials with Resistencia a la tracción of 210.0 - 265.0 MPa | H44 | EN 573-3 | Sheet, Strip | Transverse |
20.0 °C | 210.0 - 265.0 MPa Show Material materials with Resistencia a la tracción of 210.0 - 265.0 MPa | H44 | EN 573-3, EN 1396 | Sheet, Strip, Plate, Foil, Welded Tube | ||
20.0 °C | 220.0 - 265.0 MPa Show Material materials with Resistencia a la tracción of 220.0 - 265.0 MPa | H44 | EN 573-3 | Flat | ||
20.0 °C | 225.0 - 265.0 MPa Show Material materials with Resistencia a la tracción of 225.0 - 265.0 MPa | H44 | EN 573-3, EN 541 | Sheet, Strip, Plate, Foil, Welded Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H44 | EN 573-3 | Sheet, Strip | |
Coeficiente de dilatación térmica | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube |
-50.0 °C | 2.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.15e-05 1/K | H44 | EN 573-3 | Sheet, Strip | |
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
20 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
20 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
100.0 °C | 2.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.32e-05 1/K | H44 | EN 573-3 | Sheet, Strip | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
200 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
200.0 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
300 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
300.0 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
Conductividad térmica | 160.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 180.0 W/(m·K) | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
163 W/(m·K) Show Material materials with Conductividad térmica of 163 W/(m·K) | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 160.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 190.0 W/(m·K) | H44 | EN 573-3 | Sheet, Strip | |
Temperatura de fusión | 629.0 - 654.0 °C Show Material materials with Temperatura de fusión of 629.0 - 654.0 °C | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
630.0 - 655.0 °C Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 25000000.0 S/m | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
24000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 S/m | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 20000000.0 - 24000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 24000000.0 S/m | H44 | EN 573-3 | Sheet, Strip | |
Resistividad eléctrica | 4e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 4.35e-08 Ω·m | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.17e-08 Ω·m | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % | H44 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Flat, Plate, Foil, Welded Tube |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H44 | EN 573-3 | Sheet, Strip, Flat |
0.70 % Show Material materials with Hierro of 0.70 % | H44 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
Magnesio | 0.8 - 1.3 % Show Material materials with Magnesio of 0.8 - 1.3 % | H44 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Flat, Plate, Foil, Welded Tube |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | H44 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Flat, Plate, Foil, Welded Tube |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | H44 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Flat, Plate, Foil, Welded Tube |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H44 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Flat, Plate, Foil, Welded Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |