General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H19 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Flat, Strip |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Dureza Brinell | 83.0 [-] Show Material materials with Dureza Brinell of 83.0 [-] | H19 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 83.0 [-] Show Material materials with Dureza Brinell of 83.0 [-] | H19 | EN 573-3 | Flat | ||
Dureza Brinell (HBW) | 45.0 - 80.0 [-] Show Material materials with Dureza Brinell (HBW) of 45.0 - 80.0 [-] | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
Límite elástico | 60.0 - 310.0 MPa Show Material materials with Límite elástico of 60.0 - 310.0 MPa | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
240.0 MPa Show Material materials with Límite elástico of 240.0 MPa | H19 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | RP02 | ||
20.0 °C | 240.0 MPa Show Material materials with Límite elástico of 240.0 MPa | H19 | EN 573-3 | Flat | RP02 | |
20.0 °C | 240.0 MPa Show Material materials with Límite elástico of 240.0 MPa | H19 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 245.0 - 310.0 MPa Show Material materials with Límite elástico of 245.0 - 310.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 245.0 - 295.0 MPa Show Material materials with Límite elástico of 245.0 - 295.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 245.0 - 290.0 MPa Show Material materials with Límite elástico of 245.0 - 290.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 250.0 - 310.0 MPa Show Material materials with Límite elástico of 250.0 - 310.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 250.0 - 295.0 MPa Show Material materials with Límite elástico of 250.0 - 295.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 250.0 - 290.0 MPa Show Material materials with Límite elástico of 250.0 - 290.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 270.0 - 310.0 MPa Show Material materials with Límite elástico of 270.0 - 310.0 MPa | H19 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | RP02 | |
20.0 °C | 270.0 - 295.0 MPa Show Material materials with Límite elástico of 270.0 - 295.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 270.0 - 290.0 MPa Show Material materials with Límite elástico of 270.0 - 290.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
Módulo de cizallamiento | 26.0 GPa Show Material materials with Módulo de cizallamiento of 26.0 GPa | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
20.0 °C | 25.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 27.0 GPa | H19 | EN 573-3 | Sheet, Flat | ||
Módulo elástico | 68.6 GPa Show Material materials with Módulo elástico of 68.6 GPa | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 155.0 - 330.0 MPa Show Material materials with Resistencia a la tracción of 155.0 - 330.0 MPa | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H19 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |||
20.0 °C | 260.0 - 330.0 MPa Show Material materials with Resistencia a la tracción of 260.0 - 330.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 260.0 - 300.0 MPa Show Material materials with Resistencia a la tracción of 260.0 - 300.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 260.0 - 310.0 MPa Show Material materials with Resistencia a la tracción of 260.0 - 310.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H19 | EN 573-3 | Flat | ||
20.0 °C | 270.0 - 330.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 330.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 270.0 - 300.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 300.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 270.0 - 310.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 310.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H19 | EN 573-3 | Flat | Transverse | |
20.0 °C | 290.0 - 330.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 330.0 MPa | H19 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 290.0 - 300.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 300.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 290.0 - 310.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 310.0 MPa | H19 | EN 573-3 | Sheet | ||
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H19 | EN 573-3 | Sheet, Flat | ||
Coeficiente de dilatación térmica | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.15e-05 1/K | H19 | EN 573-3 | Sheet, Flat | ||
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
20 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.32e-05 1/K | H19 | EN 573-3 | Sheet, Flat | ||
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | 20-100°C | |
200 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
200.0 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
300 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
300.0 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
Conductividad térmica | 160.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 180.0 W/(m·K) | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
163 W/(m·K) Show Material materials with Conductividad térmica of 163 W/(m·K) | H19 | EN 573-3, EN 485, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Strip | |||
20.0 °C | 160.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 190.0 W/(m·K) | H19 | EN 573-3 | Sheet, Flat | ||
Temperatura de fusión | 629.0 - 654.0 °C Show Material materials with Temperatura de fusión of 629.0 - 654.0 °C | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
630.0 - 655.0 °C Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 25000000.0 S/m | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
24000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 S/m | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 20000000.0 - 24000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 24000000.0 S/m | H19 | EN 573-3 | Sheet, Flat | |
Resistividad eléctrica | 4e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 4.35e-08 Ω·m | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
4.0999999999999997e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.0999999999999997e-08 Ω·m | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.17e-08 Ω·m | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % | H19 | EN 573-3, EN 485, EN 541 | Sheet, Flat, Strip, Plate, Foil, Welded Tube |
0.25 % Show Material materials with Cobre of 0.25 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H19 | EN 573-3 | Sheet, Flat |
0.70 % Show Material materials with Hierro of 0.70 % | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
0.7 % Show Material materials with Hierro of 0.7 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Magnesio | 0.8 - 1.3 % Show Material materials with Magnesio of 0.8 - 1.3 % | H19 | EN 573-3, EN 485, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Flat, Strip, Plate, Foil, Welded Tube, Strip |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | H19 | EN 573-3, EN 485, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Flat, Strip, Plate, Foil, Welded Tube, Strip |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | H19 | EN 573-3, EN 485, EN 541 | Sheet, Flat, Strip, Plate, Foil, Welded Tube |
0.3 % Show Material materials with Silicona of 0.3 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H19 | EN 573-3, EN 485, EN 541 | Sheet, Flat, Strip, Plate, Foil, Welded Tube |
0.25 % Show Material materials with Zinc of 0.25 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Intermediate transformation/interior use; Heat exchangers: Fins; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Food can: Body, Lids; Semi-rigid and corrugated: Smooth wall | |
Brazing | Very Good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |