General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Flat, Sheet, Strip |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Dureza Brinell | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | O | EN 573-3 | Flat | ||
Dureza Brinell (HBW) | 45.0 - 80.0 [-] Show Material materials with Dureza Brinell (HBW) of 45.0 - 80.0 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
Elongación | -196.0 °C | 38.0 % Show Material materials with Elongación of 38.0 % | O | EN 573-3 | ||
-80.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | O | EN 573-3 | |||
-28.0 °C | 26.0 % Show Material materials with Elongación of 26.0 % | O | EN 573-3 | |||
1 % Show Material materials with Elongación of 1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | A50 | ||
13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A100 | ||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A50 | ||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3 | Flat | ||
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | O | EN 573-3 | |||
100.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | O | EN 573-3 | |||
150.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3 | |||
200.0 °C | 55.0 % Show Material materials with Elongación of 55.0 % | O | EN 573-3 | |||
260.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | O | EN 573-3 | |||
315.0 °C | 80.0 % Show Material materials with Elongación of 80.0 % | O | EN 573-3 | |||
370.0 °C | 90.0 % Show Material materials with Elongación of 90.0 % | O | EN 573-3 | |||
Límite elástico | -196.0 °C | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | O | EN 573-3 | RP02 | |
-80.0 °C | 75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | O | EN 573-3 | RP02 | ||
-28.0 °C | 70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | O | EN 573-3 | RP02 | ||
60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | RP02 | ||
60.0 - 310.0 MPa Show Material materials with Límite elástico of 60.0 - 310.0 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |||
20.0 °C | 60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3 | Flat | RP02 | |
20.0 °C | 60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | O | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | O | EN 573-3 | RP02 | ||
100.0 °C | 70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | O | EN 573-3 | RP02 | ||
150.0 °C | 70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | O | EN 573-3 | RP02 | ||
200.0 °C | 65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | O | EN 573-3 | RP02 | ||
260.0 °C | 50.0 MPa Show Material materials with Límite elástico of 50.0 MPa | O | EN 573-3 | RP02 | ||
315.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | RP02 | ||
370.0 °C | 20.0 MPa Show Material materials with Límite elástico of 20.0 MPa | O | EN 573-3 | RP02 | ||
Módulo de cizallamiento | 26.0 GPa Show Material materials with Módulo de cizallamiento of 26.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
20.0 °C | 25.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 27.0 GPa | O | EN 573-3 | Flat | ||
Módulo elástico | 68.6 GPa Show Material materials with Módulo elástico of 68.6 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | -196.0 °C | 290.0 MPa Show Material materials with Resistencia a la tracción of 290.0 MPa | O | EN 573-3 | ||
-80.0 °C | 190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | O | EN 573-3 | |||
-28.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | O | EN 573-3 | |||
155.0 - 330.0 MPa Show Material materials with Resistencia a la tracción of 155.0 - 330.0 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |||
20.0 °C | 155.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 155.0 - 200.0 MPa | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
20.0 °C | 155.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 155.0 - 200.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | O | EN 573-3 | |||
100.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | O | EN 573-3 | |||
150.0 °C | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | O | EN 573-3 | |||
200.0 °C | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | O | EN 573-3 | |||
260.0 °C | 70.0 MPa Show Material materials with Resistencia a la tracción of 70.0 MPa | O | EN 573-3 | |||
315.0 °C | 50.0 MPa Show Material materials with Resistencia a la tracción of 50.0 MPa | O | EN 573-3 | |||
370.0 °C | 35.0 MPa Show Material materials with Resistencia a la tracción of 35.0 MPa | O | EN 573-3 | |||
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |||
1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Ángulo de flexión a 90° | 1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | O | EN 573-3 | Flat | ||
Coeficiente de dilatación térmica | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.15e-05 1/K | O | EN 573-3 | Flat | ||
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
20 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.32e-05 1/K | O | EN 573-3 | Flat | ||
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | 20-100°C | |
200 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
200.0 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
300 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
300.0 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | ||
Conductividad térmica | 160.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 180.0 W/(m·K) | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
163 W/(m·K) Show Material materials with Conductividad térmica of 163 W/(m·K) | O | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Strip | |||
20.0 °C | 160.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 190.0 W/(m·K) | O | EN 573-3 | Flat | ||
Temperatura de fusión | 629.0 - 654.0 °C Show Material materials with Temperatura de fusión of 629.0 - 654.0 °C | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
630.0 - 655.0 °C Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 25000000.0 S/m | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
24000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 S/m | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 20000000.0 - 24000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 24000000.0 S/m | O | EN 573-3 | Flat | |
Resistividad eléctrica | 4e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 4.35e-08 Ω·m | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
4.0999999999999997e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.0999999999999997e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.17e-08 Ω·m | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % | O | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Welded Tube |
0.25 % Show Material materials with Cobre of 0.25 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-3 | Flat |
0.70 % Show Material materials with Hierro of 0.70 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Magnesio | 0.8 - 1.3 % Show Material materials with Magnesio of 0.8 - 1.3 % | O | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Flat, Strip, Sheet, Plate, Foil, Welded Tube, Strip |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | O | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Flat, Strip, Sheet, Plate, Foil, Welded Tube, Strip |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | O | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Welded Tube |
0.3 % Show Material materials with Silicona of 0.3 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Welded Tube |
0.25 % Show Material materials with Zinc of 0.25 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Intermediate transformation/interior use; Heat exchangers: Fins; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Food can: Body, Lids; Semi-rigid and corrugated: Smooth wall | |
Brazing | Very Good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |