General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Foil, Rod, Flat, Seamless Tube, Tube, Wire |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 75.0 MPa Show Material materials with Bending Fatigue Strength of 75.0 MPa | H18 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | |
Dureza Brinell | 58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 55.0 [-] Show Material materials with Dureza Brinell of 55.0 [-] | H18 | EN 573-3 | Rod, Tube | ||
20.0 °C | 58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | H18 | EN 573-3 | Flat | ||
Dureza Brinell (HBW) | 62 [-] Show Material materials with Dureza Brinell (HBW) of 62 [-] | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
Elongación | -196.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | H18 | EN 573-3 | ||
-80.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | H18 | EN 573-3 | |||
-20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H18 | EN 573-3 | |||
1.0 % Show Material materials with Elongación of 1.0 % | H18 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
1.0 - 2.0 % Show Material materials with Elongación of 1.0 - 2.0 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | A50 | ||
2.0 % Show Material materials with Elongación of 2.0 % | H18 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
2.0 % Show Material materials with Elongación of 2.0 % | H18 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
3.0 % Show Material materials with Elongación of 3.0 % | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
3.0 % Show Material materials with Elongación of 3.0 % | H18 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H18 | EN 573-3 | Foil | A100 | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H18 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H18 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H18 | EN 573-3 | Seamless Tube | ||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H18 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H18 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H18 | EN 573-3 | Rod, Tube | ||
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H18 | EN 573-3 | Wire | A100 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H18 | EN 573-3 | |||
100.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H18 | EN 573-3 | |||
150.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H18 | EN 573-3 | |||
200.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | H18 | EN 573-3 | |||
260.0 °C | 60.0 % Show Material materials with Elongación of 60.0 % | H18 | EN 573-3 | |||
320.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | H18 | EN 573-3 | |||
370.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | H18 | EN 573-3 | |||
Límite elástico | -196.0 °C | 232.0 MPa Show Material materials with Límite elástico of 232.0 MPa | H18 | EN 573-3 | RP02 | |
-80.0 °C | 204.0 MPa Show Material materials with Límite elástico of 204.0 MPa | H18 | EN 573-3 | RP02 | ||
-20.0 °C | 197.0 MPa Show Material materials with Límite elástico of 197.0 MPa | H18 | EN 573-3 | RP02 | ||
145.0 MPa Show Material materials with Límite elástico of 145.0 MPa | H18 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
160.0 MPa Show Material materials with Límite elástico of 160.0 MPa | H18 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
165.0 MPa Show Material materials with Límite elástico of 165.0 MPa | H18 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
165 MPa Show Material materials with Límite elástico of 165 MPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
170.0 MPa Show Material materials with Límite elástico of 170.0 MPa | H18 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
20.0 °C | 145.0 MPa Show Material materials with Límite elástico of 145.0 MPa | H18 | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 160.0 MPa Show Material materials with Límite elástico of 160.0 MPa | H18 | EN 573-3 | Foil | RP02 | |
20.0 °C | 165.0 MPa Show Material materials with Límite elástico of 165.0 MPa | H18 | EN 573-3 | Wire, Flat | RP02 | |
20.0 °C | 165.0 MPa Show Material materials with Límite elástico of 165.0 MPa | H18 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 170.0 MPa Show Material materials with Límite elástico of 170.0 MPa | H18 | EN 573-3 | Seamless Tube | RP02 | |
20.0 °C | 190.0 MPa Show Material materials with Límite elástico of 190.0 MPa | H18 | EN 573-3 | RP02 | ||
100.0 °C | 148.0 MPa Show Material materials with Límite elástico of 148.0 MPa | H18 | EN 573-3 | RP02 | ||
150.0 °C | 113.0 MPa Show Material materials with Límite elástico of 113.0 MPa | H18 | EN 573-3 | RP02 | ||
200.0 °C | 63.0 MPa Show Material materials with Límite elástico of 63.0 MPa | H18 | EN 573-3 | RP02 | ||
260.0 °C | 28.0 MPa Show Material materials with Límite elástico of 28.0 MPa | H18 | EN 573-3 | RP02 | ||
320.0 °C | 17.0 MPa Show Material materials with Límite elástico of 17.0 MPa | H18 | EN 573-3 | RP02 | ||
370.0 °C | 13.0 MPa Show Material materials with Límite elástico of 13.0 MPa | H18 | EN 573-3 | RP02 | ||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.1 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.1 - 26.5 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
Módulo elástico | -270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Foil, Rod, Flat, Seamless Tube, Tube, Wire | |
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Módulo elástico of 69.0 - 69.5 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Módulo elástico of 69.5 - 70.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | -196.0 °C | 298.0 MPa Show Material materials with Resistencia a la tracción of 298.0 MPa | H18 | EN 573-3 | ||
-80.0 °C | 225.0 MPa Show Material materials with Resistencia a la tracción of 225.0 MPa | H18 | EN 573-3 | |||
-20.0 °C | 214.0 MPa Show Material materials with Resistencia a la tracción of 214.0 MPa | H18 | EN 573-3 | |||
170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | H18 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | H18 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
185 MPa Show Material materials with Resistencia a la tracción of 185 MPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | H18 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | H18 | EN 573-3 | Wire | ||
20.0 °C | 175.0 MPa Show Material materials with Resistencia a la tracción of 175.0 MPa | H18 | EN 573-3 | Foil | ||
20.0 °C | 175.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 175.0 - 230.0 MPa | H18 | EN 573-3 | Foil | ||
20.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | H18 | EN 573-3 | Rod, Tube | ||
20.0 °C | 185.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 185.0 - 230.0 MPa | H18 | EN 573-3, EN 546 | Foil, Strip, Sheet, Plate, Bar, Rod, Tube | ||
20.0 °C | 185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | H18 | EN 573-3 | Foil, Flat | ||
20.0 °C | 185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | H18 | EN 573-3 | Flat | Transverse | |
20.0 °C | 190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | H18 | EN 573-3 | Seamless Tube | ||
20.0 °C | 204.0 MPa Show Material materials with Resistencia a la tracción of 204.0 MPa | H18 | EN 573-3 | |||
100.0 °C | 183.0 MPa Show Material materials with Resistencia a la tracción of 183.0 MPa | H18 | EN 573-3 | |||
150.0 °C | 163.0 MPa Show Material materials with Resistencia a la tracción of 163.0 MPa | H18 | EN 573-3 | |||
200.0 °C | 98.0 MPa Show Material materials with Resistencia a la tracción of 98.0 MPa | H18 | EN 573-3 | |||
260.0 °C | 53.0 MPa Show Material materials with Resistencia a la tracción of 53.0 MPa | H18 | EN 573-3 | |||
320.0 °C | 28.0 MPa Show Material materials with Resistencia a la tracción of 28.0 MPa | H18 | EN 573-3 | |||
370.0 °C | 21.0 MPa Show Material materials with Resistencia a la tracción of 21.0 MPa | H18 | EN 573-3 | |||
Ángulo de flexión a 90° | 1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
3.0 °/t Show Material materials with Ángulo de flexión a 90° of 3.0 °/t | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Calor específico of 892.0 - 893.0 J/(kg·K) | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 892.0 J/(kg·K) Show Material materials with Calor específico of 892.0 J/(kg·K) | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
100 °C | 0.000025 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000025 1/K | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | 20-100°C | |
Conductividad térmica | 176 W/(m·K) Show Material materials with Conductividad térmica of 176 W/(m·K) | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Seamless Tube, Wire | ||
20.0 °C | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | ||
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 28000000.0 S/m | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Seamless Tube, Wire |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 29000000.0 S/m | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | |
Resistividad eléctrica | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.57e-08 - 4.55e-08 Ω·m | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
4.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-08 Ω·m | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.1e-08 Ω·m | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.5e-08 Ω·m | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 Ω·m | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 - 4.5e-08 Ω·m | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar |
0.1 % Show Material materials with Cobre of 0.1 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar |
0.1 % Show Material materials with Cromo of 0.1 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H18 | EN 573-3 | Foil, Rod, Flat, Seamless Tube, Tube, Wire |
0.70 % Show Material materials with Hierro of 0.70 % | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
0.7 % Show Material materials with Hierro of 0.7 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar |
0.3 % Show Material materials with Magnesio of 0.3 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar, Coil, Sheet |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar |
0.5 % Show Material materials with Silicona of 0.5 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H18 | EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754 | Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar |
0.2 % Show Material materials with Zinc of 0.2 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Lithography; Heat exchangers: Fins, Heat exchangers; Tubes: Flexible tube, Pipes; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Components: Automotive fins, Heat exchangers | |
Brazing | hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |