General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | |
2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Flat, Coil, Sheet |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Dureza Brinell | 29.0 [-] Show Material materials with Dureza Brinell of 29.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 29.0 [-] Show Material materials with Dureza Brinell of 29.0 [-] | O | EN 573-3 | Flat | ||
Dureza Brinell (HBW) | 29 [-] Show Material materials with Dureza Brinell (HBW) of 29 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
Límite elástico | 40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | RP02 | |
40 MPa Show Material materials with Límite elástico of 40 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
20.0 °C | 40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | EN 573-3 | Sheet, Strip, Flat | RP02 Transverse | |
20.0 °C | 40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | EN 573-3 | Sheet, Strip, Flat | RP02 | |
Módulo de cizallamiento | 26.0 GPa Show Material materials with Módulo de cizallamiento of 26.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | ||
69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 100.0 - 155.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 155.0 MPa | O | EN 573-3 | Sheet, Strip, Flat | Transverse |
20.0 °C | 100.0 - 155.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 155.0 MPa | O | EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Coil, Sheet, Flat | ||
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 - 920.0 J/(kg·K) Show Material materials with Calor específico of 893.0 - 920.0 J/(kg·K) | Typical for Wrought 3000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | 20-100°C | |
Conductividad térmica | 160.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 190.0 W/(m·K) | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | ||
172 W/(m·K) Show Material materials with Conductividad térmica of 172 W/(m·K) | O | EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Coil, Sheet | |||
20.0 °C | 180.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 180.0 - 190.0 W/(m·K) | O | EN 573-3 | Sheet, Strip, Flat | ||
Temperatura de fusión | 635.0 - 655.0 °C Show Material materials with Temperatura de fusión of 635.0 - 655.0 °C | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | ||
640.0 - 655.0 °C Show Material materials with Temperatura de fusión of 640.0 - 655.0 °C | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 26000000.0 S/m | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | |
26000000.0 S/m Show Material materials with Conductividad eléctrica of 26000000.0 S/m | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 25000000.0 - 27000000.0 S/m Show Material materials with Conductividad eléctrica of 25000000.0 - 27000000.0 S/m | O | EN 573-3 | Sheet, Strip, Flat | |
Resistividad eléctrica | 3.7999999999999996e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.7999999999999996e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
3.85e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 Ω·m | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | ||
3.85e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 - 4.35e-08 Ω·m | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | O | EN 573-3, EN 1396, EN 485 | Sheet, Strip, Flat, Plate |
0.3 % Show Material materials with Cobre of 0.3 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Cromo | 0.2 % Show Material materials with Cromo of 0.2 % | O | EN 573-3, EN 1396, EN 485 | Sheet, Strip, Flat, Plate |
0.2 % Show Material materials with Cromo of 0.2 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-3 | Sheet, Strip, Flat |
0.70 % Show Material materials with Hierro of 0.70 % | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate | |
0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Magnesio | 0.2 - 0.8 % Show Material materials with Magnesio of 0.2 - 0.8 % | O | EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Flat, Plate, Coil, Sheet |
Manganeso | 0.3 - 0.8 % Show Material materials with Manganeso of 0.3 - 0.8 % | O | EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Strip, Flat, Plate, Coil, Sheet |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | O | EN 573-3, EN 1396, EN 485 | Sheet, Strip, Flat, Plate |
0.6 % Show Material materials with Silicona of 0.6 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | O | EN 573-3, EN 1396, EN 485 | Sheet, Strip, Flat, Plate |
Zinc | 0.4 % Show Material materials with Zinc of 0.4 % | O | EN 573-3, EN 1396, EN 485 | Sheet, Strip, Flat, Plate |
0.4 % Show Material materials with Zinc of 0.4 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | Good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Heat exchangers: Fins; Closures: Short cups; Semi-rigid and corrugated: Pet food | |
Brazing | hard brazing (with flux/ without flux): very good - acceptable / very good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Surface Finish | Mill finish | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |