General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H28 | EN 573-3 | Sheet, Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Dureza Brinell | 61.0 [-] Show Material materials with Dureza Brinell of 61.0 [-] | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 61.0 [-] Show Material materials with Dureza Brinell of 61.0 [-] | H28 | EN 573-3 | Flat | ||
Módulo de cizallamiento | 25.0 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 26.0 GPa | Typical for Wrought 3000 Series Aluminium | ||||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 190.0 - 240.0 MPa Show Material materials with Resistencia a la tracción of 190.0 - 240.0 MPa | H28 | EN 573-3 | Sheet | ||
20.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | H28 | EN 573-3 | Flat | ||
20.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | H28 | EN 573-3 | Flat | Transverse |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 - 920.0 J/(kg·K) Show Material materials with Calor específico of 893.0 - 920.0 J/(kg·K) | Typical for Wrought 3000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
Conductividad térmica | 160.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 190.0 W/(m·K) | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
172 W/(m·K) Show Material materials with Conductividad térmica of 172 W/(m·K) | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
20.0 °C | 180.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 180.0 - 190.0 W/(m·K) | H28 | EN 573-3 | Sheet, Flat | ||
Temperatura de fusión | 635.0 - 655.0 °C Show Material materials with Temperatura de fusión of 635.0 - 655.0 °C | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
640.0 - 655.0 °C Show Material materials with Temperatura de fusión of 640.0 - 655.0 °C | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 26000000.0 S/m | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
26000000.0 S/m Show Material materials with Conductividad eléctrica of 26000000.0 S/m | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 25000000.0 - 27000000.0 S/m Show Material materials with Conductividad eléctrica of 25000000.0 - 27000000.0 S/m | H28 | EN 573-3 | Sheet, Flat | |
Resistividad eléctrica | 3.85e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 Ω·m | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 - 4.35e-08 Ω·m | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | H28 | EN 573-3, EN 485 | Sheet, Flat, Strip, Plate |
Cromo | 0.2 % Show Material materials with Cromo of 0.2 % | H28 | EN 573-3, EN 485 | Sheet, Flat, Strip, Plate |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H28 | EN 573-3 | Sheet, Flat |
0.70 % Show Material materials with Hierro of 0.70 % | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
Magnesio | 0.2 - 0.8 % Show Material materials with Magnesio of 0.2 - 0.8 % | H28 | EN 573-3, EN 485 | Sheet, Flat, Strip, Plate |
Manganeso | 0.3 - 0.8 % Show Material materials with Manganeso of 0.3 - 0.8 % | H28 | EN 573-3, EN 485 | Sheet, Flat, Strip, Plate |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | H28 | EN 573-3, EN 485 | Sheet, Flat, Strip, Plate |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | H28 | EN 573-3, EN 485 | Sheet, Flat, Strip, Plate |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H28 | EN 573-3 | Sheet |
0.4 % Show Material materials with Zinc of 0.4 % | H28 | EN 573-3, EN 485 | Sheet, Flat, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Brazing | hard brazing (with flux/ without flux): very good - acceptable / very good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |