General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | F | EN 573-3, EN 570 | Strip, Sheet, Plate |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | |||
Dureza Brinell | 25.0 [-] Show Material materials with Dureza Brinell of 25.0 [-] | F | EN 573-3, EN 570 | Strip, Sheet, Plate | |
Módulo de cizallamiento | 25.0 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 26.0 GPa | Typical for Wrought 3000 Series Aluminium | |||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | F | EN 573-3, EN 570 | Strip, Sheet, Plate | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 893.0 - 920.0 J/(kg·K) Show Material materials with Calor específico of 893.0 - 920.0 J/(kg·K) | Typical for Wrought 3000 Series Aluminium |
Coeficiente de dilatación térmica | 2.2e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 - 2.4e-05 1/K | Typical for Wrought 3000 Series Aluminium |
Conductividad térmica | 154.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 154.0 - 193.0 W/(m·K) | Typical for Wrought 3000 Series Aluminium |
Temperatura de fusión | 629.0 - 654.0 °C Show Material materials with Temperatura de fusión of 629.0 - 654.0 °C | Typical for Wrought 3000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 23000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 29000000.0 S/m | Typical for Wrought 3000 Series Aluminium |
Resistividad eléctrica | 3.4e-08 - 4.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.2e-08 Ω·m | Typical for Wrought 3000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | F | EN 573-3, EN 570 | Strip, Sheet, Plate |
Hierro | 0.45 % Show Material materials with Hierro of 0.45 % | F | EN 573-3, EN 570 | Strip, Sheet, Plate |
Magnesio | 0.1 % Show Material materials with Magnesio of 0.1 % | F | EN 573-3, EN 570 | Strip, Sheet, Plate |
Manganeso | 0.4 - 0.8 % Show Material materials with Manganeso of 0.4 - 0.8 % | F | EN 573-3, EN 570 | Strip, Sheet, Plate |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | F | EN 573-3, EN 570 | Strip, Sheet, Plate |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | F | EN 573-3, EN 570 | Strip, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |