General
Property | Value | Comment |
---|---|---|
Densidad | 2.65 - 2.71 g/cm³ Show Material materials with Densidad of 2.65 - 2.71 g/cm³ | Typical for Cast 4xx.x Series Aluminium |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 4xx.x Series Aluminium | ||||
Dureza Brinell | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | F | EN 1706, EN 13195 | Casting | ||
20.0 °C | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | F | EN 1706 | |||
Módulo elástico | 71.0 - 75.0 GPa Show Material materials with Módulo elástico of 71.0 - 75.0 GPa | Typical for Cast 4xx.x Series Aluminium | ||||
Resistencia a la tracción | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | F | EN 1706, EN 13195 | Casting | ||
170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | F | EN 1706, EN 13195 | Casting | |||
20.0 °C | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | F | EN 1706 | |||
20.0 °C | 170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | F | EN 1706 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 963.0 J/(kg·K) Show Material materials with Calor específico of 963.0 J/(kg·K) | Typical for Cast 4xx.x Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | F | EN 1706, EN 13195 | Casting | |
100.0 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | F | EN 1706, EN 13195 | Casting | ||
100 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | F | EN 1706, EN 13195 | Casting | ||
Conductividad térmica | 20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 - 160.0 W/(m·K) | F | EN 1706, EN 13195 | Casting | |
Temperatura de fusión | 565.0 - 630.0 °C Show Material materials with Temperatura de fusión of 565.0 - 630.0 °C | Typical for Cast 4xx.x Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 19000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 25000000.0 S/m | F | EN 1706, EN 13195 | Casting |
Resistividad eléctrica | 4e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 5.26e-08 Ω·m | F | EN 1706, EN 13195 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 95.05 % Show Material materials with Aluminio of 95.05 % | F | EN 1706 | |
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | F | EN 1706, EN 13195 | Casting |
Estaño | 0.05 % Show Material materials with Estaño of 0.05 % | F | EN 1706, EN 13195 | Casting |
Hierro | 0.6 % Show Material materials with Hierro of 0.6 % | F | EN 1706 | |
0.60 % Show Material materials with Hierro of 0.60 % | F | EN 1706, EN 13195 | Casting | |
Magnesio | 0.45 - 0.65 % Show Material materials with Magnesio of 0.45 - 0.65 % | F | EN 1706, EN 13195 | Casting |
Manganeso | 0.3 - 0.5 % Show Material materials with Manganeso of 0.3 - 0.5 % | F | EN 1706, EN 13195 | Casting |
Níquel | 0.05 % Show Material materials with Níquel of 0.05 % | F | EN 1706, EN 13195 | Casting |
0.15 % Show Material materials with Níquel of 0.15 % | F | EN 1706 | ||
Plomo | 0.05 % Show Material materials with Plomo of 0.05 % | F | EN 1706, EN 13195 | Casting |
Silicona | 1.6 - 2.4 % Show Material materials with Silicona of 1.6 - 2.4 % | F | EN 1706, EN 13195 | Casting |
Titanio | 0.05 - 0.2 % Show Material materials with Titanio of 0.05 - 0.2 % | F | EN 1706, EN 13195 | Casting |
0.15 - 0.2 % Show Material materials with Titanio of 0.15 - 0.2 % | F | EN 1706 | ||
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | F | EN 1706, EN 13195 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good | |
Corrosion properties | general: good | |
General machinability | after thermal treatment: acceptable, as cast: good | |
Processing methods | permanent mould casting, separately cast test sample |