General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube |
Medidas
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Espesor | 0.2 mm Show Material materials with Espesor of 0.2 mm | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | 0.2 mm | Coil, Sheet, Strip |
3.0 mm Show Material materials with Espesor of 3.0 mm | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | 3.0 mm | Coil, Sheet, Strip |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 75.0 MPa Show Material materials with Bending Fatigue Strength of 75.0 MPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Dureza Brinell | 48.0 [-] Show Material materials with Dureza Brinell of 48.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 48.0 [-] Show Material materials with Dureza Brinell of 48.0 [-] | H14 | EN 573-3 | Flat | ||
Dureza Brinell (HBW) | 48 [-] Show Material materials with Dureza Brinell (HBW) of 48 [-] | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | |
2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
2.0 - 3.0 % Show Material materials with Elongación of 2.0 - 3.0 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | A50 | ||
3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A100 | ||
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3 | Foil | A50 | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Rod, Tube | ||
Límite elástico | 110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | |
120.0 MPa Show Material materials with Límite elástico of 120.0 MPa | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | ||
120 MPa Show Material materials with Límite elástico of 120 MPa | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
125.0 MPa Show Material materials with Límite elástico of 125.0 MPa | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | ||
20.0 °C | 110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | H14 | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 120.0 MPa Show Material materials with Límite elástico of 120.0 MPa | H14 | EN 573-3 | Flat | RP02 | |
20.0 °C | 120.0 MPa Show Material materials with Límite elástico of 120.0 MPa | H14 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 125.0 MPa Show Material materials with Límite elástico of 125.0 MPa | H14 | EN 573-3 | Foil | RP02 | |
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 145.0 - 190.0 MPa Show Material materials with Resistencia a la tracción of 145.0 - 190.0 MPa | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 145.0 - 185.0 MPa Show Material materials with Resistencia a la tracción of 145.0 - 185.0 MPa | H14 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Flat, Strip, Sheet, Plate, Tube, Welded Tube, Bar, Coil, Sheet, Strip | ||
20.0 °C | 145.0 - 185.0 MPa Show Material materials with Resistencia a la tracción of 145.0 - 185.0 MPa | H14 | EN 573-3 | Flat | Transverse | |
Ángulo de flexión a 180° | 1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
2.0 °/t Show Material materials with Ángulo de flexión a 180° of 2.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
2.5 °/t Show Material materials with Ángulo de flexión a 180° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
1 °/t Show Material materials with Ángulo de flexión a 90° of 1 °/t | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 897.0 J/(kg·K) Show Material materials with Calor específico of 897.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Coeficiente de dilatación térmica | 20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | 20-100°C | |
Conductividad térmica | 200 W/(m·K) Show Material materials with Conductividad térmica of 200 W/(m·K) | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
201 W/(m·K) Show Material materials with Conductividad térmica of 201 W/(m·K) | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
20.0 °C | 201.0 W/(m·K) Show Material materials with Conductividad térmica of 201.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Temperatura de fusión | 630.0 - 655.0 °C Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 30000000.0 S/m Show Material materials with Conductividad eléctrica of 30000000.0 S/m | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
Resistividad eléctrica | 3.33e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.33e-08 Ω·m | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 3.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-08 Ω·m | H14 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Rod, Flat, Foil, Tube, Coil, Sheet, Strip |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H14 | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Cobre of 0.2 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
0.2 % Show Material materials with Cobre of 0.2 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
0.1 % Show Material materials with Cromo of 0.1 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Hierro | 0.45 % Show Material materials with Hierro of 0.45 % | H14 | EN 573-3 | Rod, Tube |
0.7 % Show Material materials with Hierro of 0.7 % | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
0.70 % Show Material materials with Hierro of 0.70 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
0.7 % Show Material materials with Hierro of 0.7 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Magnesio | 0.5 - 1.1 % Show Material materials with Magnesio of 0.5 - 1.1 % | H14 | EN 573-3, EN 485, EN 683, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar, Coil, Sheet, Strip |
0.7 - 1.1 % Show Material materials with Magnesio of 0.7 - 1.1 % | H14 | EN 573-3 | Rod, Tube | |
Manganeso | 0.15 % Show Material materials with Manganeso of 0.15 % | H14 | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Manganeso of 0.2 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
0.2 % Show Material materials with Manganeso of 0.2 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
0.3 % Show Material materials with Silicona of 0.3 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H14 | EN 573-3 | Rod, Tube |
0.25 % Show Material materials with Zinc of 0.25 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
0.25 % Show Material materials with Zinc of 0.25 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Heat exchangers: Fins, General applications; Cosmetics: Cosmetics pieces; Automotive trim: Interior trim; Components: Automotive fins, Heat exchangers | |
Brazing | hard brazing (with flux/ without flux): acceptable / sufficient, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (O) |