General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.64 g/cm³ Show Material materials with Densidad of 2.64 g/cm³ | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | |
20.0 °C | 2.64 g/cm³ Show Material materials with Densidad of 2.64 g/cm³ | O | EN 573-3 | Rod, Tube, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 65.0 [-] Show Material materials with Dureza Brinell of 65.0 [-] | O | EN 573-3 | Rod, Tube | |
Elongación | 13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3, EN 755 | Rod, Tube, Wire | A50 | |
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 754 | Rod, Tube, Wire | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 755 | Rod, Tube, Wire | A100 | ||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 754 | Rod, Tube, Wire | A100 | ||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 1301 | Rod, Tube, Wire | |||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Wire | A100 | |
20.0 °C | 28.0 % Show Material materials with Elongación of 28.0 % | O | EN 573-3 | |||
60.0 °C | 28.0 % Show Material materials with Elongación of 28.0 % | O | EN 573-3 | |||
100.0 °C | 32.0 % Show Material materials with Elongación of 32.0 % | O | EN 573-3 | |||
140.0 °C | 40.0 % Show Material materials with Elongación of 40.0 % | O | EN 573-3 | |||
180.0 °C | 52.0 % Show Material materials with Elongación of 52.0 % | O | EN 573-3 | |||
240.0 °C | 64.0 % Show Material materials with Elongación of 64.0 % | O | EN 573-3 | |||
300.0 °C | 100.0 % Show Material materials with Elongación of 100.0 % | O | EN 573-3 | |||
360.0 °C | 104.0 % Show Material materials with Elongación of 104.0 % | O | EN 573-3 | |||
Módulo de cizallamiento | 20.0 °C | 27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | O | EN 573-3 | Rod, Tube, Wire | |
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 250.0 - 310.0 MPa Show Material materials with Resistencia a la tracción of 250.0 - 310.0 MPa | O | EN 573-3, EN 1715-3 | Rod, Tube, Wire | ||
320.0 MPa Show Material materials with Resistencia a la tracción of 320.0 MPa | O | EN 573-3, EN 1301 | Rod, Tube, Wire | |||
20.0 °C | 250.0 - 320.0 MPa Show Material materials with Resistencia a la tracción of 250.0 - 320.0 MPa | O | EN 573-3, EN 754, EN 755 | Rod, Tube, Wire | ||
20.0 °C | 250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 280.0 MPa Show Material materials with Resistencia a la tracción of 280.0 MPa | O | EN 573-3 | |||
20.0 °C | 320.0 MPa Show Material materials with Resistencia a la tracción of 320.0 MPa | O | EN 573-3 | Wire | ||
100.0 °C | 275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | O | EN 573-3 | |||
140.0 °C | 235.0 MPa Show Material materials with Resistencia a la tracción of 235.0 MPa | O | EN 573-3 | |||
180.0 °C | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | O | EN 573-3 | |||
240.0 °C | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | O | EN 573-3 | |||
300.0 °C | 100.0 MPa Show Material materials with Resistencia a la tracción of 100.0 MPa | O | EN 573-3 | |||
360.0 °C | 55.0 MPa Show Material materials with Resistencia a la tracción of 55.0 MPa | O | EN 573-3 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 904.0 J/(kg·K) Show Material materials with Calor específico of 904.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
20.0 °C | 904.0 J/(kg·K) Show Material materials with Calor específico of 904.0 J/(kg·K) | O | EN 573-3 | Rod, Tube, Wire | ||
Coeficiente de dilatación térmica | -50 °C | 2.2499999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2499999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | |
-50.0 °C | 2.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.25e-05 1/K | O | EN 573-3 | Rod, Tube, Wire | ||
20 °C | 2.2499999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2499999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
20 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
20 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
20 °C | 2.61e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.61e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
100 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
100.0 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
200 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
200.0 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
300 °C | 2.61e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.61e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
300.0 °C | 2.61e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.61e-05 1/K | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
Conductividad térmica | 20.0 °C | 110.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 - 140.0 W/(m·K) | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | |
Temperatura de fusión | 575.0 - 630.0 °C Show Material materials with Temperatura de fusión of 575.0 - 630.0 °C | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | ||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 15000000.0 - 19000000.0 S/m Show Material materials with Conductividad eléctrica of 15000000.0 - 19000000.0 S/m | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Resistividad eléctrica | 5.26e-08 - 6.67e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.26e-08 - 6.67e-08 Ω·m | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Cromo | 0.2 % Show Material materials with Cromo of 0.2 % | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | O | EN 573-3 | Rod, Tube, Wire |
0.50 % Show Material materials with Hierro of 0.50 % | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire | |
Magnesio | 4.5 - 5.6 % Show Material materials with Magnesio of 4.5 - 5.6 % | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Manganeso | 0.1 - 0.6 % Show Material materials with Manganeso of 0.1 - 0.6 % | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | O | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | Rod, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): poor, Deep drawing / upsetting (Condition) good (O) / good (O) |