General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
20.0 °C | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H13 | EN 573-3 | Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
20.0 °C | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | H13 | EN 573-3 | Tube | ||
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | |
7.0 % Show Material materials with Elongación of 7.0 % | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H13 | EN 573-3 | Tube | A50 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H13 | EN 573-3 | Tube | ||
Módulo de cizallamiento | 20.0 °C | 26.5 Show Material materials with Módulo de cizallamiento of 26.5 | H13 | EN 573-3 | Tube | |
Módulo elástico | -270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H13 | EN 573-3 | Tube | |
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H13 | EN 573-3 | Tube | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H13 | EN 573-3 | Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H13 | EN 573-3 | Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H13 | EN 573-3 | Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H13 | EN 573-3 | Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H13 | EN 573-3 | Tube | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H13 | EN 573-3 | Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 225.0 - 280.0 MPa Show Material materials with Resistencia a la tracción of 225.0 - 280.0 MPa | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 879.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3699999999999997e-05 1/K | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3699999999999997e-05 1/K | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Conductividad térmica | 20.0 °C | 140.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 - 180.0 W/(m·K) | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube | |
Temperatura de fusión | 620.0 - 650.0 °C Show Material materials with Temperatura de fusión of 620.0 - 650.0 °C | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | H13 | EN 573-3 | Tube | Long | |
150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 20000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 25000000.0 S/m | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Resistividad eléctrica | 4e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 5e-08 Ω·m | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | H13 | EN 573-3 | Tube |
0.50 % Show Material materials with Hierro of 0.50 % | H13 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
Magnesio | 1.6 - 2.5 % Show Material materials with Magnesio of 1.6 - 2.5 % | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Manganeso | 0.5 - 1.1 % Show Material materials with Manganeso of 0.5 - 1.1 % | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H13 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |