General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate |
2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 54.0 [-] Show Material materials with Dureza Brinell of 54.0 [-] | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 54.0 [-] Show Material materials with Dureza Brinell of 54.0 [-] | H34 | EN 573-3 | Flat | ||
Dureza Brinell (HBW) | 54 [-] Show Material materials with Dureza Brinell (HBW) of 54 [-] | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
Límite elástico | 135.0 MPa Show Material materials with Límite elástico of 135.0 MPa | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | RP02 | |
135 MPa Show Material materials with Límite elástico of 135 MPa | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |||
20.0 °C | 135.0 MPa Show Material materials with Límite elástico of 135.0 MPa | H34 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 135.0 MPa Show Material materials with Límite elástico of 135.0 MPa | H34 | EN 573-3 | Flat | RP02 | |
Módulo de cizallamiento | 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
Módulo elástico | 68.6 GPa Show Material materials with Módulo elástico of 68.6 GPa | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 175.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 175.0 - 215.0 MPa | H34 | EN 573-3 | Flat | Transverse |
20.0 °C | 175.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 175.0 - 215.0 MPa | H34 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Coil, Sheet, Strip, Flat | ||
Ángulo de flexión a 180° | 1 °/t Show Material materials with Ángulo de flexión a 180° of 1 °/t | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
2.0 °/t Show Material materials with Ángulo de flexión a 180° of 2.0 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 879.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | 20-100°C | |
Conductividad térmica | 170.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 190.0 W/(m·K) | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
192 W/(m·K) Show Material materials with Conductividad térmica of 192 W/(m·K) | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |||
193 W/(m·K) Show Material materials with Conductividad térmica of 193 W/(m·K) | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Temperatura de fusión | 620.0 - 650.0 °C Show Material materials with Temperatura de fusión of 620.0 - 650.0 °C | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
625.0 - 650.0 °C Show Material materials with Temperatura de fusión of 625.0 - 650.0 °C | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 26000000.0 S/m | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate |
29000000.0 S/m Show Material materials with Conductividad eléctrica of 29000000.0 S/m | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
Resistividad eléctrica | 3.4e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 Ω·m | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
3.45e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 Ω·m | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 - 4.35e-08 Ω·m | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.2 % Show Material materials with Cobre of 0.2 % | H34 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.2 % Show Material materials with Cobre of 0.2 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H34 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.1 % Show Material materials with Cromo of 0.1 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H34 | EN 573-3 | Flat |
0.70 % Show Material materials with Hierro of 0.70 % | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
0.7 % Show Material materials with Hierro of 0.7 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Magnesio | 1.1 - 1.8 % Show Material materials with Magnesio of 1.1 - 1.8 % | H34 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Strip, Sheet, Plate, Coil, Sheet, Strip |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | H34 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.1 % Show Material materials with Manganeso of 0.1 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
0.3 % Show Material materials with Manganeso of 0.3 % | H34 | EN 573-3 | Flat | |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H34 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.4 % Show Material materials with Silicona of 0.4 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H34 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.25 % Show Material materials with Zinc of 0.25 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | Very Good (anodizing quality) | |
Application areas | Roofing: Single sheet, Sheets for composites/ sandwich Panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Anodizing quality; Tubes: Industrial tubes, Pipes; Food can: Body, Lids | |
Brazing | Good | |
Corrosion properties | Excellent | |
General machinability | Fair | |
Welding | Excellent | |
Workability | Very Good |