General
Property | Value | Comment |
---|---|---|
Densidad | 2.6 - 2.7 g/cm³ Show Material materials with Densidad of 2.6 - 2.7 g/cm³ | Typical for Cast 5xx.x Series Aluminium |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 - 110.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa | F | EN 1706 | Casting | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 5xx.x Series Aluminium | |||
Dureza Brinell | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | F | EN 1706 | Casting | |
Módulo elástico | 68.0 - 70.0 GPa Show Material materials with Módulo elástico of 68.0 - 70.0 GPa | Typical for Cast 5xx.x Series Aluminium | |||
Resistencia a la tracción | 250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | F | EN 1706 | Casting |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 963.0 J/(kg·K) Show Material materials with Calor específico of 963.0 J/(kg·K) | Typical for Cast 5xx.x Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | F | EN 1706 | Casting | |
100 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | F | EN 1706 | Casting | ||
Conductividad térmica | 110.0 - 130.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 - 130.0 W/(m·K) | F | EN 1706 | Casting | ||
Temperatura de fusión | 450.0 - 640.0 °C Show Material materials with Temperatura de fusión of 450.0 - 640.0 °C | Typical for Cast 5xx.x Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 14000000.0 - 16000000.0 S/m Show Material materials with Conductividad eléctrica of 14000000.0 - 16000000.0 S/m | F | EN 1706 | Casting |
Resistividad eléctrica | 6.25e-08 - 7.14e-08 Ω·m Show Material materials with Resistividad eléctrica of 6.25e-08 - 7.14e-08 Ω·m | F | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 89.83 % Show Material materials with Aluminio of 89.83 % | F | EN 1706 | |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | F | EN 1706 | Casting |
Hierro | 0.25 % Show Material materials with Hierro of 0.25 % | F | EN 1706 | |
0.25 % Show Material materials with Hierro of 0.25 % | F | EN 1706 | Casting | |
Magnesio | 4.7 - 6.0 % Show Material materials with Magnesio of 4.7 - 6.0 % | F | EN 1706 | Casting |
Manganeso | 0.4 - 0.8 % Show Material materials with Manganeso of 0.4 - 0.8 % | F | EN 1706 | Casting |
Silicona | 1.8 - 2.6 % Show Material materials with Silicona of 1.8 - 2.6 % | F | EN 1706 | Casting |
Titanio | 0.25 % Show Material materials with Titanio of 0.25 % | F | EN 1706 | Casting |
Zinc | 0.07 % Show Material materials with Zinc of 0.07 % | F | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: excellent | |
General machinability | as cast: excellent | |
Processing methods | pressure die casting, separately cast test sample |