General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Densidad | 2.65 g/cm³ Show Material materials with Densidad of 2.65 g/cm³ | F | EN 1706 | |
20.0 °C | 2.65 g/cm³ Show Material materials with Densidad of 2.65 g/cm³ | F | DIN 1725-2, EN 1676, EN 1706 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 - 110.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa | F | EN 1706 | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Dureza Brinell | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | F | EN 1706 | ||
55.0 [-] Show Material materials with Dureza Brinell of 55.0 [-] | F | EN 1706 | |||
20.0 °C | 50.0 - 60.0 [-] Show Material materials with Dureza Brinell of 50.0 - 60.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 60.0 [-] Show Material materials with Dureza Brinell of 60.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 60.0 - 80.0 [-] Show Material materials with Dureza Brinell of 60.0 - 80.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | F | EN 1706 | A50 | |
2.5 % Show Material materials with Elongación of 2.5 % | F | EN 1706 | A50 | ||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 2.0 - 6.0 % Show Material materials with Elongación of 2.0 - 6.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
Módulo de cizallamiento | 2.8 GPa Show Material materials with Módulo de cizallamiento of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Módulo elástico | 74.0 GPa Show Material materials with Módulo elástico of 74.0 GPa | F | EN 1706 | ||
20.0 °C | 74.0 GPa Show Material materials with Módulo elástico of 74.0 GPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Resistencia a la tracción | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | F | EN 1706 | ||
180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | F | EN 1706 | |||
20.0 °C | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 160.0 - 210.0 MPa Show Material materials with Resistencia a la tracción of 160.0 - 210.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 180.0 - 240.0 MPa Show Material materials with Resistencia a la tracción of 180.0 - 240.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Resistencia al cizallamiento | 20.0 °C | 137.0 MPa Show Material materials with Resistencia al cizallamiento of 137.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 910.0 J/(kg·K) Show Material materials with Calor específico of 910.0 J/(kg·K) | F | EN 1706 | |
20.0 °C | 910.0 J/(kg·K) Show Material materials with Calor específico of 910.0 J/(kg·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Coeficiente de dilatación térmica | 20 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | F | EN 1706 |
100 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | F | EN 1706 | |
200.0 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
Conductividad térmica | 150.0 - 170.0 W/(m·K) Show Material materials with Conductividad térmica of 150.0 - 170.0 W/(m·K) | F | EN 1706 | |
20.0 °C | 130.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 190.0 W/(m·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Temperatura de fusión | 550.0 - 600.0 °C Show Material materials with Temperatura de fusión of 550.0 - 600.0 °C | F | EN 1706 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Conductividad eléctrica | 19000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 25000000.0 S/m | F | EN 1706 | |
20.0 °C | 17000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 26000000.0 S/m | F | DIN 1725-2, EN 1676, EN 1706 | |
Resistividad eléctrica | 4e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 5.26e-08 Ω·m | F | EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 87.2 % Show Material materials with Aluminio of 87.2 % | F | DIN 1725-2, EN 1676, EN 1706 |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | F | DIN 1725-2, EN 1676, EN 1706 |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
0.50 % Show Material materials with Hierro of 0.50 % | F | EN 1706 | |
Magnesio | 0.2 - 0.5 % Show Material materials with Magnesio of 0.2 - 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Manganeso | 0.001 - 0.4 % Show Material materials with Manganeso of 0.001 - 0.4 % | F | DIN 1725-2, EN 1676, EN 1706 |
Silicona | 9.0 - 11.0 % Show Material materials with Silicona of 9.0 - 11.0 % | F | DIN 1725-2, EN 1676, EN 1706 |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | F | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | F | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: good | |
General machinability | after thermal treatment: good to acceptable, as cast: good | |
Processing methods | permanent mould casting, sample taken from casting or cast on |