General
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 5xx.x Series Aluminium | |||
Dureza Brinell | 55.0 [-] Show Material materials with Dureza Brinell of 55.0 [-] | F | EN 1706 | ||
60.0 [-] Show Material materials with Dureza Brinell of 60.0 [-] | F | EN 1706 | |||
20.0 °C | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 55.0 [-] Show Material materials with Dureza Brinell of 55.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 55.0 - 70.0 [-] Show Material materials with Dureza Brinell of 55.0 - 70.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 60.0 - 75.0 [-] Show Material materials with Dureza Brinell of 60.0 - 75.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
Elongación | 3.0 % Show Material materials with Elongación of 3.0 % | F | EN 1706 | A50 | |
4.0 % Show Material materials with Elongación of 4.0 % | F | EN 1706 | A50 | ||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 3.0 - 8.0 % Show Material materials with Elongación of 3.0 - 8.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 4.0 - 10.0 % Show Material materials with Elongación of 4.0 - 10.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | F | EN 1706 | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Resistencia a la tracción | 160.0 MPa Show Material materials with Resistencia a la tracción of 160.0 MPa | F | EN 1706 | ||
170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | F | EN 1706 | |||
180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | F | EN 1706 | |||
20.0 °C | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 160.0 - 220.0 MPa Show Material materials with Resistencia a la tracción of 160.0 - 220.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 180.0 - 240.0 MPa Show Material materials with Resistencia a la tracción of 180.0 - 240.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 940.0 J/(kg·K) Show Material materials with Calor específico of 940.0 J/(kg·K) | F | EN 1706 | |
20.0 °C | 940.0 J/(kg·K) Show Material materials with Calor específico of 940.0 J/(kg·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Coeficiente de dilatación térmica | 20 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | F | EN 1706 |
100 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | F | EN 1706 | |
200.0 °C | 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
Conductividad térmica | 20.0 °C | 110.0 - 130.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 - 130.0 W/(m·K) | F | DIN 1725-2, EN 1676, EN 1706 |
Temperatura de fusión | 560.0 - 640.0 °C Show Material materials with Temperatura de fusión of 560.0 - 640.0 °C | F | EN 1706 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Conductividad eléctrica | 15000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 15000000.0 - 21000000.0 S/m | F | EN 1706 | |
20.0 °C | 15000000.0 - 20000000.0 S/m Show Material materials with Conductividad eléctrica of 15000000.0 - 20000000.0 S/m | F | DIN 1725-2, EN 1676, EN 1706 | |
Resistividad eléctrica | 4.76e-08 - 6.67e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 6.67e-08 Ω·m | F | EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 92.6 % Show Material materials with Aluminio of 92.6 % | F | DIN 1725-2, EN 1676, EN 1706 |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | F | DIN 1725-2, EN 1676, EN 1706 |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
0.50 % Show Material materials with Hierro of 0.50 % | F | EN 1706 | |
Magnesio | 4.5 - 5.5 % Show Material materials with Magnesio of 4.5 - 5.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Manganeso | 0.001 - 0.4 % Show Material materials with Manganeso of 0.001 - 0.4 % | F | DIN 1725-2, EN 1676, EN 1706 |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Titanio | 0.001 - 0.2 % Show Material materials with Titanio of 0.001 - 0.2 % | F | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | F | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: excellent | |
Corrosion properties | general: excellent | |
General machinability | after thermal treatment: excellent | |
Processing methods | permanent mould casting, sample taken from casting |