General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Densidad | 2.65 g/cm³ Show Material materials with Densidad of 2.65 g/cm³ | F | EN 1706 | |
20.0 °C | 2.65 g/cm³ Show Material materials with Densidad of 2.65 g/cm³ | F | DIN 1725-2, EN 1676, EN 1706 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Dureza Brinell | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | F | EN 1706 | ||
20.0 °C | 60.0 - 100.0 [-] Show Material materials with Dureza Brinell of 60.0 - 100.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | F | EN 1706 | A50 | |
20.0 °C | 1.0 - 3.0 % Show Material materials with Elongación of 1.0 - 3.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
Módulo de cizallamiento | 2.8 GPa Show Material materials with Módulo de cizallamiento of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Módulo elástico | 76.0 GPa Show Material materials with Módulo elástico of 76.0 GPa | F | EN 1706 | ||
20.0 °C | 76.0 GPa Show Material materials with Módulo elástico of 76.0 GPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Resistencia a la tracción | 240.0 MPa Show Material materials with Resistencia a la tracción of 240.0 MPa | F | EN 1706 | ||
20.0 °C | 220.0 - 300.0 MPa Show Material materials with Resistencia a la tracción of 220.0 - 300.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 890.0 J/(kg·K) Show Material materials with Calor específico of 890.0 J/(kg·K) | F | EN 1706 | |
20.0 °C | 890.0 J/(kg·K) Show Material materials with Calor específico of 890.0 J/(kg·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Coeficiente de dilatación térmica | 20 °C | 1.9999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9999999999999998e-05 1/K | F | EN 1706 |
20 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
100 °C | 1.9999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9999999999999998e-05 1/K | F | EN 1706 | |
200.0 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
200 °C | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
Conductividad térmica | 120.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 150.0 W/(m·K) | F | EN 1706 | |
20.0 °C | 120.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 140.0 W/(m·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Temperatura de fusión | 530.0 - 580.0 °C Show Material materials with Temperatura de fusión of 530.0 - 580.0 °C | F | EN 1706 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Conductividad eléctrica | 15000000.0 - 20000000.0 S/m Show Material materials with Conductividad eléctrica of 15000000.0 - 20000000.0 S/m | F | EN 1706 | |
20.0 °C | 16000000.0 - 20000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 20000000.0 S/m | F | DIN 1725-2, EN 1676, EN 1706 | |
Resistividad eléctrica | 5e-08 - 6.67e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 - 6.67e-08 Ω·m | F | EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 81.9 % Show Material materials with Aluminio of 81.9 % | F | DIN 1725-2, EN 1676, EN 1706 |
Cobre | 1.2 % Show Material materials with Cobre of 1.2 % | F | DIN 1725-2, EN 1676, EN 1706 |
Estaño | 0.1 % Show Material materials with Estaño of 0.1 % | F | DIN 1725-2, EN 1676, EN 1706 |
Hierro | 1.2 % Show Material materials with Hierro of 1.2 % | F | DIN 1725-2, EN 1676, EN 1706 |
1.20 % Show Material materials with Hierro of 1.20 % | F | EN 1706 | |
Magnesio | 0.4 % Show Material materials with Magnesio of 0.4 % | F | DIN 1725-2, EN 1676, EN 1706 |
Manganeso | 0.1 - 0.5 % Show Material materials with Manganeso of 0.1 - 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Níquel | 0.2 % Show Material materials with Níquel of 0.2 % | F | DIN 1725-2, EN 1676, EN 1706 |
Plomo | 0.2 % Show Material materials with Plomo of 0.2 % | F | DIN 1725-2, EN 1676, EN 1706 |
Silicona | 10.5 - 13.5 % Show Material materials with Silicona of 10.5 - 13.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | F | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.5 % Show Material materials with Zinc of 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: acceptable | |
General machinability | after thermal treatment: acceptable | |
Processing methods | pressure die casting, separately cast test sample |