DIN 1725-1 Grade 3.0515 H16

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMn1 is an Al-Mn alloy, which belongs to the nature-hard aluminum materials. Mn increases the strength compared with pure aluminium, but it does not impair the corrosion resistance. The alloy belongs to the nature-hard aluminum materials. A strength increase can only occur by cold forming. It is very well formable, very well corrosion resistant and weldable. In these characteristics it resembles the pure aluminium, but with the attainable strength it exceeds this. The alloy AlMn1 has a increased heat resistance compared with pure aluminium, as result of the of the Mn-additive (inhibits recrystallisation). Application: In the building industry for roofings, as outer skin of buildings, in the apparatus and tank construction as heat exchanger (bank of tubes, profiles, gilled pipes, sheet metals), for radiators, air conditioning systems, pipings for compressed gas tanks, for tanks according VdTUEV Werkstoffblaetter, as antennas for radio relay link and satellite communication (mirror) for technical flow pressed parts, for solid rivets, for generally metal-describe, in food industry (including commercial devices), in the construction of vehicles (including tank cars) and as packing (sheet metal packings generally).

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM,AluKey.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

2.73 g/cm³

Show Material materials with Densidad of 2.73 g/cm³

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

20.0 °C

2.73 g/cm³

Show Material materials with Densidad of 2.73 g/cm³

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Dureza Brinell

51.0 [-]

Show Material materials with Dureza Brinell of 51.0 [-]

H16

EN 573-3, EN 485

20.0 °C

40.0 [-]

Show Material materials with Dureza Brinell of 40.0 [-]

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Tube

20.0 °C

45.0 [-]

Show Material materials with Dureza Brinell of 45.0 [-]

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod

Elongación

1.0 %

Show Material materials with Elongación of 1.0 %

H16

EN 573-3, EN 485, EN 683

A50

2.0 %

Show Material materials with Elongación of 2.0 %

H16

EN 573-3, EN 485

A50

3.0 %

Show Material materials with Elongación of 3.0 %

H16

EN 573-3, EN 1592

A100

3.0 %

Show Material materials with Elongación of 3.0 %

H16

EN 573-3, EN 754

A50

4.0 %

Show Material materials with Elongación of 4.0 %

H16

EN 573-3, EN 754

A100

20.0 °C

3.0 %

Show Material materials with Elongación of 3.0 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

A10

20.0 °C

4.0 %

Show Material materials with Elongación of 4.0 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

Módulo de cizallamiento

26.1 GPa

Show Material materials with Módulo de cizallamiento of 26.1 GPa

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

20.0 °C

24.0 - 26.5 GPa

Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

Módulo elástico

69.5 GPa

Show Material materials with Módulo elástico of 69.5 GPa

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Módulo elástico of 60.0 - 65.0 GPa

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Resistencia a la tracción

150.0 - 200.0 MPa

Show Material materials with Resistencia a la tracción of 150.0 - 200.0 MPa

H16

EN 573-3, EN 683

160.0 - 200.0 MPa

Show Material materials with Resistencia a la tracción of 160.0 - 200.0 MPa

H16

EN 573-3, EN 485, EN 683

160.0 - 195.0 MPa

Show Material materials with Resistencia a la tracción of 160.0 - 195.0 MPa

H16

EN 573-3, EN 754

170.0 MPa

Show Material materials with Resistencia a la tracción of 170.0 MPa

H16

EN 573-3, EN 1592

20.0 °C

160.0 MPa

Show Material materials with Resistencia a la tracción of 160.0 MPa

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

Ángulo de flexión a 180°

2.0 °/t

Show Material materials with Ángulo de flexión a 180° of 2.0 °/t

H16

EN 573-3, EN 485

2.5 °/t

Show Material materials with Ángulo de flexión a 180° of 2.5 °/t

H16

EN 573-3, EN 485

Ángulo de flexión a 90°

1.0 °/t

Show Material materials with Ángulo de flexión a 90° of 1.0 °/t

H16

EN 573-3, EN 485

1.5 °/t

Show Material materials with Ángulo de flexión a 90° of 1.5 °/t

H16

EN 573-3, EN 485

2.0 °/t

Show Material materials with Ángulo de flexión a 90° of 2.0 °/t

H16

EN 573-3, EN 485

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShape

Calor específico

893.0 J/(kg·K)

Show Material materials with Calor específico of 893.0 J/(kg·K)

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

20.0 °C

893.0 J/(kg·K)

Show Material materials with Calor específico of 893.0 J/(kg·K)

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

Coeficiente de dilatación térmica

20 °C

2.35e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

100 °C

2.35e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

Conductividad térmica

20.0 °C

160.0 - 200.0 W/(m·K)

Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K)

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1592, EN 485, EN 683, EN 754

Rod, Tube

Temperatura de fusión

645.0 - 655.0 °C

Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShape

Conductividad eléctrica

20.0 °C

22000000.0 - 28000000.0 S/m

Show Material materials with Conductividad eléctrica of 22000000.0 - 28000000.0 S/m

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1592, EN 485, EN 683, EN 754

Rod, Tube

Resistividad eléctrica

3.57e-08 - 4.55e-08 Ω·m

Show Material materials with Resistividad eléctrica of 3.57e-08 - 4.55e-08 Ω·m

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

Chemical properties

PropertyValueConditionRelated StandardsShape

Cobre

0.1 %

Show Material materials with Cobre of 0.1 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1592, EN 485, EN 683, EN 754

Rod, Tube

Cromo

0.1 %

Show Material materials with Cromo of 0.1 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1592, EN 485, EN 683, EN 754

Rod, Tube

Hierro

0.7 %

Show Material materials with Hierro of 0.7 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

0.70 %

Show Material materials with Hierro of 0.70 %

H16

EN 573-3, EN 1592, EN 485, EN 683, EN 754

Magnesio

0.3 %

Show Material materials with Magnesio of 0.3 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1592, EN 485, EN 683, EN 754

Rod, Tube

Manganeso

0.9 - 1.5 %

Show Material materials with Manganeso of 0.9 - 1.5 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1592, EN 485, EN 683, EN 754

Rod, Tube

Silicona

0.5 %

Show Material materials with Silicona of 0.5 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1592, EN 485, EN 683, EN 754

Rod, Tube

Titanio

0.1

Show Material materials with Titanio of 0.1

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4

Rod, Tube

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H16

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1592, EN 485, EN 683, EN 754

Rod, Tube

Technological properties

Property
Workability

Good workability.