General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H112 | EN 573-3, EN 485, EN 755 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||
Dureza Brinell | 28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | H112 | EN 573-3, EN 485 | |
34.0 [-] Show Material materials with Dureza Brinell of 34.0 [-] | H112 | EN 573-3, EN 485 | ||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H112 | EN 573-3, EN 485, EN 755 | |
Módulo elástico | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H112 | EN 573-3, EN 485, EN 755 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Resistencia a la tracción | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | H112 | EN 573-3, EN 485, EN 755 | |
110.0 MPa Show Material materials with Resistencia a la tracción of 110.0 MPa | H112 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H112 | EN 573-3, EN 485, EN 755 | |
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H112 | EN 573-3, EN 485, EN 755 |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | |
Conductividad térmica | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H112 | EN 573-3, EN 485, EN 755 | |
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H112 | EN 573-3, EN 485, EN 755 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 22000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 28000000.0 S/m | H112 | EN 573-3, EN 485, EN 755 |
Resistividad eléctrica | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.57e-08 - 4.55e-08 Ω·m | H112 | EN 573-3, EN 485, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H112 | EN 573-3, EN 485, EN 755 |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H112 | EN 573-3, EN 485, EN 755 |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | H112 | EN 573-3, EN 485, EN 755 |
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | H112 | EN 573-3, EN 485, EN 755 |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | H112 | EN 573-3, EN 485, EN 755 |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | H112 | EN 573-3, EN 485, EN 755 |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H112 | EN 573-3, EN 485, EN 755 |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |