DIN 1725-1 Grade 3.0526 H14

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMn1Mg1 has similar properties like AlMn1, however it reaches higher strength (to F 26). It has also relatively high strength in the soft condition, but it is well cold fomrable. The alloy belongs to the nature-hard aluminum materials. A strength increase can be achieved, not by a purposeful heat treatment only by cold forming. It is very well warm and cold transformable and is suitable to the deep-drawing (no lappet formation). The alloy is very corrosion and sea water-steadily. The main field of application, the packing, determines the kind of semi-finished material standardized according to DIN 1788 and DIN 1745 (sheet metal and strip). Application: In the packing (DIN 59606) for cans (dose lower parts, abgestreckte doses), breaking covers and catches of all kinds. In the building industry for roofings (usually profile boards), claddings as well as for roll shutter and roll gates.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM,AluKey.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

2.72 g/cm³

Show Material materials with Densidad of 2.72 g/cm³

H14

EN 573-3, EN 1592, EN 485

20.0 °C

2.72 g/cm³

Show Material materials with Densidad of 2.72 g/cm³

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Dureza Brinell

67.0 [-]

Show Material materials with Dureza Brinell of 67.0 [-]

H14

EN 573-3, EN 485

20.0 °C

65.0 [-]

Show Material materials with Dureza Brinell of 65.0 [-]

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Elongación

1.0 %

Show Material materials with Elongación of 1.0 %

H14

EN 573-3, EN 485

A50

2.0 %

Show Material materials with Elongación of 2.0 %

H14

EN 573-3, EN 485

A50

3.0 %

Show Material materials with Elongación of 3.0 %

H14

EN 573-3, EN 485

A50

6.0 %

Show Material materials with Elongación of 6.0 %

H14

EN 573-3, EN 1592

A100

20.0 °C

3.0 %

Show Material materials with Elongación of 3.0 %

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

A10

20.0 °C

4.0 %

Show Material materials with Elongación of 4.0 %

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Módulo de cizallamiento

20.0 °C

25.0 - 27.0 GPa

Show Material materials with Módulo de cizallamiento of 25.0 - 27.0 GPa

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Módulo elástico

69.0 GPa

Show Material materials with Módulo elástico of 69.0 GPa

H14

EN 573-3, EN 1592, EN 485

70.0 GPa

Show Material materials with Módulo elástico of 70.0 GPa

H14

EN 573-3, EN 1592, EN 485

20.0 °C

65.0 - 71.0 GPa

Show Material materials with Módulo elástico of 65.0 - 71.0 GPa

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Resistencia a la tracción

220.0 MPa

Show Material materials with Resistencia a la tracción of 220.0 MPa

H14

EN 573-3, EN 1592

220.0 - 265.0 MPa

Show Material materials with Resistencia a la tracción of 220.0 - 265.0 MPa

H14

EN 573-3, EN 485

20.0 °C

220.0 - 260.0 MPa

Show Material materials with Resistencia a la tracción of 220.0 - 260.0 MPa

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Ángulo de flexión a 180°

2.5 °/t

Show Material materials with Ángulo de flexión a 180° of 2.5 °/t

H14

EN 573-3, EN 485

Ángulo de flexión a 90°

0.5 °/t

Show Material materials with Ángulo de flexión a 90° of 0.5 °/t

H14

EN 573-3, EN 485

1.0 °/t

Show Material materials with Ángulo de flexión a 90° of 1.0 °/t

H14

EN 573-3, EN 485

1.5 °/t

Show Material materials with Ángulo de flexión a 90° of 1.5 °/t

H14

EN 573-3, EN 485

2.0 °/t

Show Material materials with Ángulo de flexión a 90° of 2.0 °/t

H14

EN 573-3, EN 485

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShape

Calor específico

893.0 J/(kg·K)

Show Material materials with Calor específico of 893.0 J/(kg·K)

H14

EN 573-3, EN 1592, EN 485

20.0 °C

893.0 J/(kg·K)

Show Material materials with Calor específico of 893.0 J/(kg·K)

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Coeficiente de dilatación térmica

-50 °C

2.1499999999999997e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K

H14

EN 573-3, EN 1592, EN 485

-50.0 °C

2.15e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.15e-05 1/K

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

20 °C

2.1499999999999997e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K

H14

EN 573-3, EN 1592, EN 485

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

20 °C

2.3899999999999998e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

20 °C

2.41e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

20 °C

2.51e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

100.0 °C

2.32e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.32e-05 1/K

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

100 °C

2.3899999999999998e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

200 °C

2.41e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

200.0 °C

2.41e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

300 °C

2.51e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

300.0 °C

2.51e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

Conductividad térmica

160.0 - 180.0 W/(m·K)

Show Material materials with Conductividad térmica of 160.0 - 180.0 W/(m·K)

H14

EN 573-3, EN 1592, EN 485

163 W/(m·K)

Show Material materials with Conductividad térmica of 163 W/(m·K)

H14

EN 573-3, EN 1592, EN 485

20.0 °C

160.0 - 190.0 W/(m·K)

Show Material materials with Conductividad térmica of 160.0 - 190.0 W/(m·K)

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Temperatura de fusión

629.0 - 654.0 °C

Show Material materials with Temperatura de fusión of 629.0 - 654.0 °C

H14

EN 573-3, EN 1592, EN 485

630.0 - 655.0 °C

Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C

H14

EN 573-3, EN 1592, EN 485

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShape

Conductividad eléctrica

23000000.0 - 25000000.0 S/m

Show Material materials with Conductividad eléctrica of 23000000.0 - 25000000.0 S/m

H14

EN 573-3, EN 1592, EN 485

24000000.0 S/m

Show Material materials with Conductividad eléctrica of 24000000.0 S/m

H14

EN 573-3, EN 1592, EN 485

20.0 °C

20000000.0 - 24000000.0 S/m

Show Material materials with Conductividad eléctrica of 20000000.0 - 24000000.0 S/m

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Resistividad eléctrica

4e-08 - 4.35e-08 Ω·m

Show Material materials with Resistividad eléctrica of 4e-08 - 4.35e-08 Ω·m

H14

EN 573-3, EN 1592, EN 485

4.17e-08 Ω·m

Show Material materials with Resistividad eléctrica of 4.17e-08 Ω·m

H14

EN 573-3, EN 1592, EN 485

Chemical properties

PropertyValueConditionRelated StandardsShape

Cobre

0.25 %

Show Material materials with Cobre of 0.25 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Hierro

0.7 %

Show Material materials with Hierro of 0.7 %

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

0.70 %

Show Material materials with Hierro of 0.70 %

H14

EN 573-3, EN 1592, EN 485

Magnesio

0.8 - 1.3 %

Show Material materials with Magnesio of 0.8 - 1.3 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Manganeso

1.0 - 1.5 %

Show Material materials with Manganeso of 1.0 - 1.5 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Silicona

0.3 %

Show Material materials with Silicona of 0.3 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12)