General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H22 | EN 573-3, EN 1592, EN 485 | ||
20.0 °C | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Dureza Brinell | 58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | H22 | EN 573-3, EN 485 | |||
20.0 °C | 55.0 [-] Show Material materials with Dureza Brinell of 55.0 [-] | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Elongación | 4.0 % Show Material materials with Elongación of 4.0 % | H22 | EN 573-3, EN 485 | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | H22 | EN 573-3, EN 485 | A50 | |||
6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3, EN 485 | A50 | |||
7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3, EN 485 | A50 | |||
8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3, EN 1592 | A100 | |||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Módulo de cizallamiento | 20.0 °C | 25.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 27.0 GPa | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H22 | EN 573-3, EN 1592, EN 485 | |||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H22 | EN 573-3, EN 1592, EN 485 | ||||
20.0 °C | 65.0 - 71.0 GPa Show Material materials with Módulo elástico of 65.0 - 71.0 GPa | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | H22 | EN 573-3, EN 1592 | |||
190.0 - 240.0 MPa Show Material materials with Resistencia a la tracción of 190.0 - 240.0 MPa | H22 | EN 573-3, EN 485 | ||||
20.0 °C | 190.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 190.0 - 230.0 MPa | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H22 | EN 573-3, EN 485 | |||
1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | H22 | EN 573-3, EN 485 | ||||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H22 | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H22 | EN 573-3, EN 485 | ||||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H22 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H22 | EN 573-3, EN 1592, EN 485 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Coeficiente de dilatación térmica | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H22 | EN 573-3, EN 1592, EN 485 | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.15e-05 1/K | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H22 | EN 573-3, EN 1592, EN 485 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H22 | EN 573-3, EN 1592, EN 485 | ||
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H22 | EN 573-3, EN 1592, EN 485 | ||
20 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H22 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
20 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H22 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H22 | EN 573-3, EN 1592, EN 485 | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.32e-05 1/K | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H22 | EN 573-3, EN 1592, EN 485 | ||
200 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H22 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
200.0 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H22 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
300 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H22 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
300.0 °C | 2.51e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K | H22 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
Conductividad térmica | 160.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 180.0 W/(m·K) | H22 | EN 573-3, EN 1592, EN 485 | ||
163 W/(m·K) Show Material materials with Conductividad térmica of 163 W/(m·K) | H22 | EN 573-3, EN 1592, EN 485 | |||
20.0 °C | 160.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 190.0 W/(m·K) | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Temperatura de fusión | 629.0 - 654.0 °C Show Material materials with Temperatura de fusión of 629.0 - 654.0 °C | H22 | EN 573-3, EN 1592, EN 485 | ||
630.0 - 655.0 °C Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C | H22 | EN 573-3, EN 1592, EN 485 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 25000000.0 S/m | H22 | EN 573-3, EN 1592, EN 485 | ||
24000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 S/m | H22 | EN 573-3, EN 1592, EN 485 | |||
20.0 °C | 20000000.0 - 24000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 24000000.0 S/m | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Resistividad eléctrica | 4e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 4.35e-08 Ω·m | H22 | EN 573-3, EN 1592, EN 485 | ||
4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.17e-08 Ω·m | H22 | EN 573-3, EN 1592, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H22 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
0.70 % Show Material materials with Hierro of 0.70 % | H22 | EN 573-3, EN 1592, EN 485 | ||
Magnesio | 0.8 - 1.3 % Show Material materials with Magnesio of 0.8 - 1.3 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |