General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||
20.0 °C | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 130.0 MPa Show Material materials with Bending Fatigue Strength of 130.0 MPa | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 83.0 [-] Show Material materials with Dureza Brinell of 83.0 [-] | H18 | EN 573-3, EN 485 | |||
20.0 °C | 85.0 [-] Show Material materials with Dureza Brinell of 85.0 [-] | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | H18 | EN 573-3, EN 485 | A50 | ||
2.0 % Show Material materials with Elongación of 2.0 % | H18 | EN 573-3, EN 485, EN 754 | A50 | |||
2.0 % Show Material materials with Elongación of 2.0 % | H18 | EN 573-3, EN 754 | A100 | |||
3.0 % Show Material materials with Elongación of 3.0 % | H18 | EN 573-3, EN 1301 | ||||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | A10 | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | ||
Módulo de cizallamiento | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H18 | EN 573-3, EN 485, EN 754 | |||
275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | H18 | EN 573-3, EN 1301 | ||||
20.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | ||
Coeficiente de dilatación térmica | -50.0 °C | 2.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.21e-05 1/K | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754, DIN 1725-1, EN 573-4, WL 3.3524-1 | Flat | ||
20 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754, DIN 1725-1, EN 573-4, WL 3.3524-1 | Flat | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754, DIN 1725-1, EN 573-4, WL 3.3524-1 | Flat | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754, DIN 1725-1, EN 573-4, WL 3.3524-1 | Flat | ||
200 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754, DIN 1725-1, EN 573-4, WL 3.3524-1 | Flat | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754, DIN 1725-1, EN 573-4, WL 3.3524-1 | Flat | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
300.0 °C | 2.57e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.57e-05 1/K | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | ||
Conductividad térmica | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||||
20.0 °C | 150.0 W/(m·K) Show Material materials with Conductividad térmica of 150.0 W/(m·K) | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | ||
Temperatura de fusión | 605.0 - 650.0 °C Show Material materials with Temperatura de fusión of 605.0 - 650.0 °C | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
607.0 - 649.0 °C Show Material materials with Temperatura de fusión of 607.0 - 649.0 °C | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 19000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 21000000.0 S/m | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||
20000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 S/m | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 21000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 S/m | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | |
Resistividad eléctrica | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.26e-08 Ω·m | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||
5e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 Ω·m | H18 | EN 573-3, EN 1301, EN 485, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754 | Flat |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754 | Flat |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat |
0.40 % Show Material materials with Hierro of 0.40 % | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754 | Flat |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754 | Flat |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754 | Flat |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754 | Flat |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |