General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | ||
20.0 °C | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 105.0 MPa Show Material materials with Bending Fatigue Strength of 105.0 MPa | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 46.0 [-] Show Material materials with Dureza Brinell of 46.0 [-] | O | EN 573-3, EN 485 | |||
47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | O | EN 573-3, EN 485 | ||||
20.0 °C | 43.0 [-] Show Material materials with Dureza Brinell of 43.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Wire | ||
20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | O | WL 3.3524-1, DIN 1725-1 | Tube | ||
20.0 °C | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Strip, Flat | ||
Elongación | -196.0 °C | 46.0 % Show Material materials with Elongación of 46.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
-80.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
-28.0 °C | 32.0 % Show Material materials with Elongación of 32.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 485 | A50 | |||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 485 | A50 | |||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 1301 | ||||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 755 | A50 | |||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 485 | A50 | |||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 755 | A100 | |||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 754 | A50 | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 485 | A100 | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 485 | A50 | |||
19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 754 | A100 | |||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Wire | A100 | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Wire | A10 | |
20.0 °C | 15.0 - 19.0 % Show Material materials with Elongación of 15.0 - 19.0 % | O | WL 3.3524-1, DIN 1725-1 | Flat | ||
20.0 °C | 16.0 - 19.0 % Show Material materials with Elongación of 16.0 - 19.0 % | O | WL 3.3524-1, DIN 1725-1 | Flat | ||
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | WL 3.3524-1, DIN 1725-1 | Tube | ||
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Strip | A10 | |
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | O | WL 3.3524-1, DIN 1725-1 | Flat | ||
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Strip | ||
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | A10 | |
20.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
100.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
150.0 °C | 50.0 % Show Material materials with Elongación of 50.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
200.0 °C | 60.0 % Show Material materials with Elongación of 60.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
260.0 °C | 80.0 % Show Material materials with Elongación of 80.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
315.0 °C | 110.0 % Show Material materials with Elongación of 110.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
370.0 °C | 130.0 % Show Material materials with Elongación of 130.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
Módulo de cizallamiento | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
20.0 °C | 27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
20.0 °C | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | -196.0 °C | 300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
-80.0 °C | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
-28.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
165.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 165.0 - 215.0 MPa | O | EN 573-3, EN 485 | ||||
170.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 230.0 MPa | O | EN 573-3, EN 754, EN 755 | ||||
225.0 MPa Show Material materials with Resistencia a la tracción of 225.0 MPa | O | EN 573-3, EN 1301 | ||||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 215.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 485 | Sheet, Strip | ||
20.0 °C | 170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Wire | ||
20.0 °C | 170.0 - 240.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 240.0 MPa | O | WL 3.3524-1, DIN 1725-1 | Tube | ||
20.0 °C | 170.0 - 220.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 220.0 MPa | O | WL 3.3524-1, DIN 1725-1 | Flat | ||
20.0 °C | 175.0 - 220.0 MPa Show Material materials with Resistencia a la tracción of 175.0 - 220.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Flat | ||
20.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
100.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
150.0 °C | 160.0 MPa Show Material materials with Resistencia a la tracción of 160.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
200.0 °C | 115.0 MPa Show Material materials with Resistencia a la tracción of 115.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
260.0 °C | 85.0 MPa Show Material materials with Resistencia a la tracción of 85.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
315.0 °C | 50.0 MPa Show Material materials with Resistencia a la tracción of 50.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
370.0 °C | 35.0 MPa Show Material materials with Resistencia a la tracción of 35.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |||
Resistencia al cizallamiento | 20.0 °C | 100.0 MPa Show Material materials with Resistencia al cizallamiento of 100.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Wire | |
Ángulo de flexión a 180° | 0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | O | EN 573-3, EN 485 | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | O | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
Coeficiente de dilatación térmica | -50.0 °C | 2.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.21e-05 1/K | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
20 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
200 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
300.0 °C | 2.57e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.57e-05 1/K | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
Conductividad térmica | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | ||||
20.0 °C | 150.0 W/(m·K) Show Material materials with Conductividad térmica of 150.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | ||
Temperatura de fusión | 605.0 - 650.0 °C Show Material materials with Temperatura de fusión of 605.0 - 650.0 °C | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
607.0 - 649.0 °C Show Material materials with Temperatura de fusión of 607.0 - 649.0 °C | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 19000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 21000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | ||
20000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | |||
20.0 °C | 21000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire | |
Resistividad eléctrica | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.26e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | ||
5e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754, EN 755 | Sheet, Flat, Strip, Wire, Tube |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754, EN 755 | Sheet, Flat, Strip, Wire, Tube |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | Sheet, Flat, Strip, Wire, Tube |
0.40 % Show Material materials with Hierro of 0.40 % | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | ||
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754, EN 755 | Sheet, Flat, Strip, Wire, Tube |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754, EN 755 | Sheet, Flat, Strip, Wire, Tube |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754, EN 755 | Sheet, Flat, Strip, Wire, Tube |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1, EN 1301, EN 485, EN 754, EN 755 | Sheet, Flat, Strip, Wire, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |