General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Dureza Brinell | 46.0 [-] Show Material materials with Dureza Brinell of 46.0 [-] | H111 | EN 573-3, EN 485 | |
47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | H111 | EN 573-3, EN 485 | ||
Módulo de cizallamiento | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | H111 | EN 573-3, EN 485, EN 754, EN 755 | |
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H111 | EN 573-3, EN 485, EN 754, EN 755 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Resistencia a la tracción | 165.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 165.0 - 215.0 MPa | H111 | EN 573-3, EN 485 | |
170.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 215.0 MPa | H111 | EN 573-3, EN 485 | ||
170.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 230.0 MPa | H111 | EN 573-3, EN 754, EN 755 | ||
Ángulo de flexión a 180° | 0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | |
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | |
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | ||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H111 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
Coeficiente de dilatación térmica | -50 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | |
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
20 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
200 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
Conductividad térmica | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | H111 | EN 573-3, EN 485, EN 754, EN 755 | |||
Temperatura de fusión | 605.0 - 650.0 °C Show Material materials with Temperatura de fusión of 605.0 - 650.0 °C | H111 | EN 573-3, EN 485, EN 754, EN 755 | ||
607.0 - 649.0 °C Show Material materials with Temperatura de fusión of 607.0 - 649.0 °C | H111 | EN 573-3, EN 485, EN 754, EN 755 | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 19000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 21000000.0 S/m | H111 | EN 573-3, EN 485, EN 754, EN 755 |
20000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 S/m | H111 | EN 573-3, EN 485, EN 754, EN 755 | |
Resistividad eléctrica | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.26e-08 Ω·m | H111 | EN 573-3, EN 485, EN 754, EN 755 |
5e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 Ω·m | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Hierro | 0.40 % Show Material materials with Hierro of 0.40 % | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H111 | EN 573-3, EN 485, EN 754, EN 755 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |