Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H14 | EN 573-3, EN 1301, EN 485, EN 754 | ||
20.0 °C | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | H14 | EN 573-3, EN 1301, EN 485, EN 754 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 72.0 [-] Show Material materials with Dureza Brinell of 72.0 [-] | H14 | EN 573-3, EN 485 | |||
20.0 °C | 73.0 [-] Show Material materials with Dureza Brinell of 73.0 [-] | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
Elongación | 3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3, EN 1301 | |||
3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3, EN 485, EN 754 | A50 | |||
4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3, EN 754 | A100 | |||
4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3, EN 485 | A50 | |||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 485 | A100 | |||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 485 | A50 | |||
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | A10 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | A10 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Módulo de cizallamiento | 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube | ||
Módulo elástico | 70.5 GPa Show Material materials with Módulo elástico of 70.5 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 68.0 - 72.0 GPa Show Material materials with Módulo elástico of 68.0 - 72.0 GPa | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 240.0 - 290.0 MPa Show Material materials with Resistencia a la tracción of 240.0 - 290.0 MPa | H14 | EN 573-3, EN 754 | |||
255.0 - 305.0 MPa Show Material materials with Resistencia a la tracción of 255.0 - 305.0 MPa | H14 | EN 573-3, EN 1301 | ||||
20.0 °C | 240.0 - 280.0 MPa Show Material materials with Resistencia a la tracción of 240.0 - 280.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Sheet, Flat, Strip | ||
20.0 °C | 250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 963.0 J/(kg·K) Show Material materials with Calor específico of 963.0 J/(kg·K) | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube | |
Coeficiente de dilatación térmica | 20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 754 | ||
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 754 | |||
100.0 °C | 2.39e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.39e-05 1/K | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube | ||
Conductividad térmica | 20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 - 160.0 W/(m·K) | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Tube | |
Temperatura de fusión | 610.0 - 640.0 °C Show Material materials with Temperatura de fusión of 610.0 - 640.0 °C | H14 | EN 573-3, EN 1301, EN 485, EN 754 | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 20000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 23000000.0 S/m | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Tube |
Resistividad eléctrica | 4.35e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.35e-08 - 5e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Tube |
Cromo | 0.3 Show Material materials with Cromo of 0.3 | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube |
0.40 % Show Material materials with Hierro of 0.40 % | H14 | EN 573-3, EN 1301, EN 485, EN 754 | ||
Magnesio | 2.6 - 3.6 % Show Material materials with Magnesio of 2.6 - 3.6 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Tube |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Tube |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Tube |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Tube |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Sheet, Flat, Strip, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good to good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |