General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H12 | EN 573-3, EN 1592, EN 485, EN 754 | ||
20.0 °C | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 130.0 MPa Show Material materials with Bending Fatigue Strength of 130.0 MPa | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 81.0 [-] Show Material materials with Dureza Brinell of 81.0 [-] | H12 | EN 573-3, EN 485 | |||
20.0 °C | 80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
Elongación | 3.0 % Show Material materials with Elongación of 3.0 % | H12 | EN 573-3, EN 485 | A50 | ||
4.0 % Show Material materials with Elongación of 4.0 % | H12 | EN 573-3, EN 485, EN 754 | A50 | |||
5.0 % Show Material materials with Elongación of 5.0 % | H12 | EN 573-3, EN 754 | A100 | |||
5.0 % Show Material materials with Elongación of 5.0 % | H12 | EN 573-3, EN 485 | A50 | |||
6.0 % Show Material materials with Elongación of 6.0 % | H12 | EN 573-3, EN 485 | A100 | |||
6.0 % Show Material materials with Elongación of 6.0 % | H12 | EN 573-3, EN 485 | A50 | |||
7.0 % Show Material materials with Elongación of 7.0 % | H12 | EN 573-3, EN 485 | A50 | |||
9.0 % Show Material materials with Elongación of 9.0 % | H12 | EN 573-3, EN 1592 | A100 | |||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
Módulo de cizallamiento | 26.7 GPa Show Material materials with Módulo de cizallamiento of 26.7 GPa | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
20.0 °C | 27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
Módulo elástico | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
20.0 °C | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H12 | EN 573-3, EN 1592, EN 754 | |||
275.0 - 335.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 335.0 MPa | H12 | EN 573-3, EN 485 | ||||
20.0 °C | 275.0 - 330.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 330.0 MPa | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
Coeficiente de dilatación térmica | -50 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | |
-50.0 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | ||
20 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | ||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | ||
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
20 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | ||
200 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
200.0 °C | 2.47e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.47e-05 1/K | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
300 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | ||
300.0 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754, DIN 1725-1, EN 573-4 | Sheet | ||
Conductividad térmica | 126 W/(m·K) Show Material materials with Conductividad térmica of 126 W/(m·K) | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
20.0 °C | 120.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 140.0 W/(m·K) | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet | ||
Temperatura de fusión | 585.0 - 641.0 °C Show Material materials with Temperatura de fusión of 585.0 - 641.0 °C | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
585.0 - 640.0 °C Show Material materials with Temperatura de fusión of 585.0 - 640.0 °C | H12 | EN 573-3, EN 1592, EN 485, EN 754 | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 18000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 S/m | H12 | EN 573-3, EN 1592, EN 485, EN 754 | ||
20.0 °C | 17000000.0 - 19000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 19000000.0 S/m | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet | |
Resistividad eléctrica | 5.26e-08 - 5.88e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.26e-08 - 5.88e-08 Ω·m | H12 | EN 573-3, EN 1592, EN 485, EN 754 | ||
5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.56e-08 Ω·m | H12 | EN 573-3, EN 1592, EN 485, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet |
0.50 % Show Material materials with Hierro of 0.50 % | H12 | EN 573-3, EN 1592, EN 485, EN 754 | ||
Magnesio | 3.5 - 4.5 % Show Material materials with Magnesio of 3.5 - 4.5 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet |
Manganeso | 0.2 - 0.7 % Show Material materials with Manganeso of 0.2 - 0.7 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |