General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 MPa | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Dureza Brinell | 40.0 [-] Show Material materials with Dureza Brinell of 40.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 35.0 [-] Show Material materials with Dureza Brinell of 35.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip, Wire | ||
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | O | EN 573-3, EN 1386 | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3, EN 1386 | A50 | |||
10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3, EN 1386 | A50 | |||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 1386 | A100 | |||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 1386, EN 755 | A50 | |||
13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3, EN 754 | A50 | |||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 755 | A100 | |||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 485 | A50 | |||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 754 | A100 | |||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 485 | A100 | |||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 485 | A50 | |||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 485 | A50 | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | A100 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | A10 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip | A10 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip | ||
Módulo de cizallamiento | 26.4 GPa Show Material materials with Módulo de cizallamiento of 26.4 GPa | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
20.0 °C | 26.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 27.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip, Wire | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
20.0 °C | 68.0 - 73.0 GPa Show Material materials with Módulo elástico of 68.0 - 73.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Resistencia a la tracción | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | O | EN 573-3, EN 1386, EN 485 | |||
155.0 MPa Show Material materials with Resistencia a la tracción of 155.0 MPa | O | EN 573-3, EN 485 | ||||
160.0 MPa Show Material materials with Resistencia a la tracción of 160.0 MPa | O | EN 573-3, EN 754, EN 755 | ||||
20.0 °C | 110.0 MPa Show Material materials with Resistencia a la tracción of 110.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | ||
20.0 °C | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip | ||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | O | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | O | EN 573-3, EN 1386 | ||||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | O | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 896.0 J/(kg·K) Show Material materials with Calor específico of 896.0 J/(kg·K) | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
Coeficiente de dilatación térmica | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
Conductividad térmica | 20.0 °C | 170.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 220.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Temperatura de fusión | 585.0 - 650.0 °C Show Material materials with Temperatura de fusión of 585.0 - 650.0 °C | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 24000000.0 - 32000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 32000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Resistividad eléctrica | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.13e-08 - 4.17e-08 Ω·m | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip, Wire |
0.50 % Show Material materials with Hierro of 0.50 % | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
Magnesio | 0.6 - 1.2 % Show Material materials with Magnesio of 0.6 - 1.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Silicona | 0.7 - 1.3 % Show Material materials with Silicona of 0.7 - 1.3 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |