General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | T6151 | EN 573-3, EN 485 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Dureza Brinell | 81.0 [-] Show Material materials with Dureza Brinell of 81.0 [-] | T6151 | EN 573-3, EN 485 | |
82.0 [-] Show Material materials with Dureza Brinell of 82.0 [-] | T6151 | EN 573-3, EN 485 | ||
Módulo de cizallamiento | 26.4 GPa Show Material materials with Módulo de cizallamiento of 26.4 GPa | T6151 | EN 573-3, EN 485 | |
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T6151 | EN 573-3, EN 485 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Resistencia a la tracción | 275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | T6151 | EN 573-3, EN 485 | |
280.0 MPa Show Material materials with Resistencia a la tracción of 280.0 MPa | T6151 | EN 573-3, EN 485 | ||
Ángulo de flexión a 90° | 2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | T6151 | EN 573-3, EN 485 | |
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | T6151 | EN 573-3, EN 485 | ||
4.0 °/t Show Material materials with Ángulo de flexión a 90° of 4.0 °/t | T6151 | EN 573-3, EN 485 | ||
5.0 °/t Show Material materials with Ángulo de flexión a 90° of 5.0 °/t | T6151 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 896.0 J/(kg·K) Show Material materials with Calor específico of 896.0 J/(kg·K) | T6151 | EN 573-3, EN 485 | |
Coeficiente de dilatación térmica | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T6151 | EN 573-3, EN 485 |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T6151 | EN 573-3, EN 485 | |
Conductividad térmica | 170.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 220.0 W/(m·K) | T6151 | EN 573-3, EN 485 | |
Temperatura de fusión | 585.0 - 650.0 °C Show Material materials with Temperatura de fusión of 585.0 - 650.0 °C | T6151 | EN 573-3, EN 485 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 24000000.0 - 32000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 32000000.0 S/m | T6151 | EN 573-3, EN 485 |
Resistividad eléctrica | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.13e-08 - 4.17e-08 Ω·m | T6151 | EN 573-3, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | T6151 | EN 573-3, EN 485 |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | T6151 | EN 573-3, EN 485 |
Hierro | 0.50 % Show Material materials with Hierro of 0.50 % | T6151 | EN 573-3, EN 485 |
Magnesio | 0.6 - 1.2 % Show Material materials with Magnesio of 0.6 - 1.2 % | T6151 | EN 573-3, EN 485 |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | T6151 | EN 573-3, EN 485 |
Silicona | 0.7 - 1.3 % Show Material materials with Silicona of 0.7 - 1.3 % | T6151 | EN 573-3, EN 485 |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | T6151 | EN 573-3, EN 485 |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | T6151 | EN 573-3, EN 485 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |