General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.85 g/cm³ Show Material materials with Densidad of 2.85 g/cm³ | T4 | EN 573-3, EN 755 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Módulo de cizallamiento | 27.3 GPa Show Material materials with Módulo de cizallamiento of 27.3 GPa | T4 | EN 573-3, EN 755 | |
Módulo elástico | 72.5 GPa Show Material materials with Módulo elástico of 72.5 GPa | T4 | EN 573-3, EN 755 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Resistencia a la tracción | 330.0 MPa Show Material materials with Resistencia a la tracción of 330.0 MPa | T4 | EN 573-3, EN 755 | |
340.0 MPa Show Material materials with Resistencia a la tracción of 340.0 MPa | T4 | EN 573-3, EN 755 | ||
370.0 MPa Show Material materials with Resistencia a la tracción of 370.0 MPa | T4 | EN 573-3, EN 755 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 860.0 J/(kg·K) Show Material materials with Calor específico of 860.0 J/(kg·K) | T4 | EN 573-3, EN 755 | |
Coeficiente de dilatación térmica | 20 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T4 | EN 573-3, EN 755 |
100 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T4 | EN 573-3, EN 755 | |
Conductividad térmica | 130.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 160.0 W/(m·K) | T4 | EN 573-3, EN 755 | |
Temperatura de fusión | 507.0 - 650.0 °C Show Material materials with Temperatura de fusión of 507.0 - 650.0 °C | T4 | EN 573-3, EN 755 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 18000000.0 - 22000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 22000000.0 S/m | T4 | EN 573-3, EN 755 |
Resistividad eléctrica | 4.55e-08 - 5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.55e-08 - 5.56e-08 Ω·m | T4 | EN 573-3, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Bismuto | 0.2 % Show Material materials with Bismuto of 0.2 % | T4 | EN 573-3, EN 755 |
Cobre | 3.3 - 4.6 % Show Material materials with Cobre of 3.3 - 4.6 % | T4 | EN 573-3, EN 755 |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | T4 | EN 573-3, EN 755 |
Estaño | 0.2 % Show Material materials with Estaño of 0.2 % | T4 | EN 573-3, EN 755 |
Hierro | 0.80 % Show Material materials with Hierro of 0.80 % | T4 | EN 573-3, EN 755 |
Magnesio | 0.4 - 1.8 % Show Material materials with Magnesio of 0.4 - 1.8 % | T4 | EN 573-3, EN 755 |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | T4 | EN 573-3, EN 755 |
Níquel | 0.2 % Show Material materials with Níquel of 0.2 % | T4 | EN 573-3, EN 755 |
Silicona | 0.8 % Show Material materials with Silicona of 0.8 % | T4 | EN 573-3, EN 755 |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | T4 | EN 573-3, EN 755 |
Zinc | 0.8 % Show Material materials with Zinc of 0.8 % | T4 | EN 573-3, EN 755 |
Technological properties
Property | ||
---|---|---|
Anodizing | Protective: poor | |
Brazing | friction soldering: sufficient | |
Corrosion properties | Seawater: poor, weathering: poor | |
Workability | Bending / Spinning (cold): sufficient / -, Deep drawing / upsetting (Condition) - / sufficient |