Pure aluminium This material is well anodically oxidizable, and possesses a good electrical and thermal conductivity. The splinter-giving workability is bad because of danger of smearing. Its mechanical strength is low, the plasticity high. The forming capacity and the chemical as well as the weather proofness are excellent. The material is well suitable for welding and braze welding. Application: Apparatus engineering, roll bond, z-bond, household devices, camp and transportation containers for the chemical, pharmaceutical and food industry, roofing, linings, arts and crafts, packing, flow pressed parts (tubes, tube, doses, bottles).

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM,AluKey.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

2.7 g/cm³

Show Material materials with Densidad of 2.7 g/cm³

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

20.0 °C

2.7 g/cm³

Show Material materials with Densidad of 2.7 g/cm³

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Dureza Brinell

18.0 [-]

Show Material materials with Dureza Brinell of 18.0 [-]

F

EN 573-3, EN 485

19.0 [-]

Show Material materials with Dureza Brinell of 19.0 [-]

F

EN 573-3, EN 570

20.0 °C

18.0 [-]

Show Material materials with Dureza Brinell of 18.0 [-]

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Elongación

20.0 °C

22.0 %

Show Material materials with Elongación of 22.0 %

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

A10

20.0 °C

25.0 %

Show Material materials with Elongación of 25.0 %

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Módulo de cizallamiento

20.0 °C

25.0 GPa

Show Material materials with Módulo de cizallamiento of 25.0 GPa

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Módulo elástico

70.0 GPa

Show Material materials with Módulo elástico of 70.0 GPa

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Módulo elástico of 60.0 - 70.0 GPa

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Resistencia a la tracción

60.0 MPa

Show Material materials with Resistencia a la tracción of 60.0 MPa

F

EN 573-3, EN 485

80.0 - 110.0 MPa

Show Material materials with Resistencia a la tracción of 80.0 - 110.0 MPa

F

EN 573-3, EN 1715-3, EN 1715-4

20.0 °C

55.0 MPa

Show Material materials with Resistencia a la tracción of 55.0 MPa

F

DIN 1712-3, EN 573-3, EN 573-4

Profile

20.0 °C

60.0 MPa

Show Material materials with Resistencia a la tracción of 60.0 MPa

F

DIN 1712-3, EN 573-3, EN 573-4

Rod, Tube

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShape

Calor específico

20.0 °C

921.0 J/(kg·K)

Show Material materials with Calor específico of 921.0 J/(kg·K)

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Coeficiente de dilatación térmica

20 °C

2.35e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

100 °C

2.35e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

Conductividad térmica

225 W/(m·K)

Show Material materials with Conductividad térmica of 225 W/(m·K)

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

20.0 °C

215.0 W/(m·K)

Show Material materials with Conductividad térmica of 215.0 W/(m·K)

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Temperatura de fusión

659.0 °C

Show Material materials with Temperatura de fusión of 659.0 °C

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShape

Conductividad eléctrica

34500000.0 - 35000000.0 S/m

Show Material materials with Conductividad eléctrica of 34500000.0 - 35000000.0 S/m

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

20.0 °C

36400000.0 - 37000000.0 S/m

Show Material materials with Conductividad eléctrica of 36400000.0 - 37000000.0 S/m

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Resistividad eléctrica

2.86e-08 - 2.9e-08 Ω·m

Show Material materials with Resistividad eléctrica of 2.86e-08 - 2.9e-08 Ω·m

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminio

99.8 %

Show Material materials with Aluminio of 99.8 %

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

Cobre

0.03 %

Show Material materials with Cobre of 0.03 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570

Profile, Rod, Tube

Galio

0.03 %

Show Material materials with Galio of 0.03 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570

Profile, Rod, Tube

Hierro

0.15 %

Show Material materials with Hierro of 0.15 %

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

0.15 %

Show Material materials with Hierro of 0.15 %

F

EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570

Magnesio

0.02 %

Show Material materials with Magnesio of 0.02 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570

Profile, Rod, Tube

Manganeso

0.02 %

Show Material materials with Manganeso of 0.02 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570

Profile, Rod, Tube

Silicona

0.15 %

Show Material materials with Silicona of 0.15 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570

Profile, Rod, Tube

Titanio

0.02 %

Show Material materials with Titanio of 0.02 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570

Profile, Rod, Tube

Zinc

0.06 %

Show Material materials with Zinc of 0.06 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570

Profile, Rod, Tube

Technological properties

Property
Anodizing

decorative: very good, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12)