General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H12 | EN 573-3, EN 485 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||
Dureza Brinell | 26.0 [-] Show Material materials with Dureza Brinell of 26.0 [-] | H12 | EN 573-3, EN 485 | |
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H12 | EN 573-3, EN 485 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||
Resistencia a la tracción | 80.0 - 120.0 MPa Show Material materials with Resistencia a la tracción of 80.0 - 120.0 MPa | H12 | EN 573-3, EN 485 | |
Ángulo de flexión a 180° | 0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | H12 | EN 573-3, EN 485 | |
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H12 | EN 573-3, EN 485 | |
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H12 | EN 573-3, EN 485 | ||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H12 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | |||
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H12 | EN 573-3, EN 485 | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H12 | EN 573-3, EN 485 | ||
Conductividad térmica | 225 W/(m·K) Show Material materials with Conductividad térmica of 225 W/(m·K) | H12 | EN 573-3, EN 485 | ||
Temperatura de fusión | 659.0 °C Show Material materials with Temperatura de fusión of 659.0 °C | H12 | EN 573-3, EN 485 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 34500000.0 - 35000000.0 S/m Show Material materials with Conductividad eléctrica of 34500000.0 - 35000000.0 S/m | H12 | EN 573-3, EN 485 |
Resistividad eléctrica | 2.86e-08 - 2.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.86e-08 - 2.9e-08 Ω·m | H12 | EN 573-3, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 99.7 % Show Material materials with Aluminio of 99.7 % | H12 | EN 573-3, EN 485 |
Cobre | 0.03 % Show Material materials with Cobre of 0.03 % | H12 | EN 573-3, EN 485 |
Hierro | 0.25 % Show Material materials with Hierro of 0.25 % | H12 | EN 573-3, EN 485 |
Magnesio | 0.03 % Show Material materials with Magnesio of 0.03 % | H12 | EN 573-3, EN 485 |
Manganeso | 0.03 % Show Material materials with Manganeso of 0.03 % | H12 | EN 573-3, EN 485 |
Silicona | 0.2 % Show Material materials with Silicona of 0.2 % | H12 | EN 573-3, EN 485 |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | H12 | EN 573-3, EN 485 |
Zinc | 0.07 % Show Material materials with Zinc of 0.07 % | H12 | EN 573-3, EN 485 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: very good, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |