General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 35.0 MPa Show Material materials with Bending Fatigue Strength of 35.0 MPa | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Dureza Brinell | 23.0 [-] Show Material materials with Dureza Brinell of 23.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 22.0 [-] Show Material materials with Dureza Brinell of 22.0 [-] | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Strip, Tube, Wire, Sheet | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | O | EN 573-3, EN 546 | A50 | ||
3.0 % Show Material materials with Elongación of 3.0 % | O | EN 573-3, EN 546 | A50 | |||
6.0 % Show Material materials with Elongación of 6.0 % | O | EN 573-3, EN 546 | A50 | |||
10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3, EN 546, EN 683 | A50 | |||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 546, EN 683 | A50 | |||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 754 | A50 | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 683 | A50 | |||
19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 754 | A100 | |||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 1396 | A50 | |||
21.0 % Show Material materials with Elongación of 21.0 % | O | EN 573-3, EN 485 | A50 | |||
22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3, EN 1396 | A50 | |||
24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3, EN 485 | A50 | |||
26.0 % Show Material materials with Elongación of 26.0 % | O | EN 573-3, EN 1396 | A50 | |||
28.0 % Show Material materials with Elongación of 28.0 % | O | EN 573-3, EN 485 | A50 | |||
30.0 % Show Material materials with Elongación of 30.0 % | O | EN 573-3, EN 485 | A100 | |||
33.0 % Show Material materials with Elongación of 33.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube, Wire | A10 | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 40.0 % Show Material materials with Elongación of 40.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Strip, Sheet | ||
100.0 °C | 45.0 % Show Material materials with Elongación of 45.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
150.0 °C | 55.0 % Show Material materials with Elongación of 55.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
200.0 °C | 65.0 % Show Material materials with Elongación of 65.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
260.0 °C | 75.0 % Show Material materials with Elongación of 75.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
315.0 °C | 80.0 % Show Material materials with Elongación of 80.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
370.0 °C | 85.0 % Show Material materials with Elongación of 85.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | |||
20.0 °C | 24.0 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.0 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Resistencia a la tracción | 40.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 40.0 - 95.0 MPa | O | EN 573-3, EN 546 | |||
45.0 - 100.0 MPa Show Material materials with Resistencia a la tracción of 45.0 - 100.0 MPa | O | EN 573-3, EN 546 | ||||
50.0 - 105.0 MPa Show Material materials with Resistencia a la tracción of 50.0 - 105.0 MPa | O | EN 573-3, EN 546 | ||||
55.0 - 105.0 MPa Show Material materials with Resistencia a la tracción of 55.0 - 105.0 MPa | O | EN 573-3, EN 546 | ||||
60.0 - 105.0 MPa Show Material materials with Resistencia a la tracción of 60.0 - 105.0 MPa | O | EN 573-3, EN 546, EN 683 | ||||
65.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 65.0 - 95.0 MPa | O | EN 573-3, EN 1396 | ||||
20.0 °C | 60.0 - 100.0 MPa Show Material materials with Resistencia a la tracción of 60.0 - 100.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 65.0 - 105.0 MPa Show Material materials with Resistencia a la tracción of 65.0 - 105.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 70.0 - 105.0 MPa Show Material materials with Resistencia a la tracción of 70.0 - 105.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4, EN 754 | Flat | ||
20.0 °C | 75.0 MPa Show Material materials with Resistencia a la tracción of 75.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube, Wire | ||
20.0 °C | 75.0 - 105.0 MPa Show Material materials with Resistencia a la tracción of 75.0 - 105.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4, EN 485 | Flat, Strip, Sheet | ||
20.0 °C | 90.0 MPa Show Material materials with Resistencia a la tracción of 90.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
100.0 °C | 70.0 MPa Show Material materials with Resistencia a la tracción of 70.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
150.0 °C | 55.0 MPa Show Material materials with Resistencia a la tracción of 55.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
200.0 °C | 40.0 MPa Show Material materials with Resistencia a la tracción of 40.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
260.0 °C | 30.0 MPa Show Material materials with Resistencia a la tracción of 30.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
315.0 °C | 20.0 MPa Show Material materials with Resistencia a la tracción of 20.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
370.0 °C | 15.0 MPa Show Material materials with Resistencia a la tracción of 15.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | |||
Ángulo de flexión a 180° | 0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Coeficiente de dilatación térmica | -50 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
-50.0 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | |||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | |||
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
100.0 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | |||
200.0 °C | 2.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.44e-05 1/K | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | |||
300.0 °C | 2.54e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.54e-05 1/K | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Conductividad térmica | 20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Conductividad térmica of 205.0 - 210.0 W/(m·K) | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Temperatura de fusión | 644.0 - 657.0 °C Show Material materials with Temperatura de fusión of 644.0 - 657.0 °C | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 33000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 33000000.0 - 34000000.0 S/m | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | ||
20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Conductividad eléctrica of 34400000.0 - 35500000.0 S/m | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Resistividad eléctrica | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.94e-08 - 3.03e-08 Ω·m | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 99.0 % Show Material materials with Aluminio of 99.0 % | O | EN 573-3, EN 1396, EN 485, EN 546, EN 683, EN 754 | |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Magnesio | 0.05 % Show Material materials with Magnesio of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Manganeso | 0.05 % Show Material materials with Manganeso of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1396, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12) |