General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H112 | EN 573-3, EN 485, EN 755 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||
Dureza Brinell | 24.0 [-] Show Material materials with Dureza Brinell of 24.0 [-] | H112 | EN 573-3, EN 485 | |
26.0 [-] Show Material materials with Dureza Brinell of 26.0 [-] | H112 | EN 573-3, EN 485 | ||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H112 | EN 573-3, EN 485, EN 755 | |
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H112 | EN 573-3, EN 485, EN 755 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||
Resistencia a la tracción | 75.0 MPa Show Material materials with Resistencia a la tracción of 75.0 MPa | H112 | EN 573-3, EN 755 | |
80.0 MPa Show Material materials with Resistencia a la tracción of 80.0 MPa | H112 | EN 573-3, EN 485 | ||
85.0 MPa Show Material materials with Resistencia a la tracción of 85.0 MPa | H112 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | |||
Coeficiente de dilatación térmica | -50 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | |
20 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | ||
20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | ||
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | ||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | ||
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | ||
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | ||
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | ||
Conductividad térmica | 205.0 - 210.0 W/(m·K) Show Material materials with Conductividad térmica of 205.0 - 210.0 W/(m·K) | H112 | EN 573-3, EN 485, EN 755 | ||
Temperatura de fusión | 644.0 - 657.0 °C Show Material materials with Temperatura de fusión of 644.0 - 657.0 °C | H112 | EN 573-3, EN 485, EN 755 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 33000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 33000000.0 - 34000000.0 S/m | H112 | EN 573-3, EN 485, EN 755 |
Resistividad eléctrica | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.94e-08 - 3.03e-08 Ω·m | H112 | EN 573-3, EN 485, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 99.0 % Show Material materials with Aluminio of 99.0 % | H112 | EN 573-3, EN 485, EN 755 |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H112 | EN 573-3, EN 485, EN 755 |
Magnesio | 0.05 % Show Material materials with Magnesio of 0.05 % | H112 | EN 573-3, EN 485, EN 755 |
Manganeso | 0.05 % Show Material materials with Manganeso of 0.05 % | H112 | EN 573-3, EN 485, EN 755 |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | H112 | EN 573-3, EN 485, EN 755 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H112 | EN 573-3, EN 485, EN 755 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12) |