General
Property | Value | Comment |
---|---|---|
Densidad | 2.65 - 2.7 g/cm³ Show Material materials with Densidad of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Dureza Brinell | 65.0 [-] Show Material materials with Dureza Brinell of 65.0 [-] | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | T51 | Pink Sheets, ASTM B108 | Casting | ||
Módulo de cizallamiento | 2.8 GPa Show Material materials with Módulo de cizallamiento of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Módulo elástico | 73.0 - 80.0 GPa Show Material materials with Módulo elástico of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Resistencia a la tracción | 170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | T51 | Pink Sheets, ASTM B108 | Casting |
Aplicaciones térmicas
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Calor específico | 960.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | |||
Coeficiente de dilatación térmica | 1.6e-05 - 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6e-05 - 2.3e-05 1/K | Typical for Cast 3xx.x Series Aluminium | |||
Conductividad térmica | 130.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 180.0 W/(m·K) | Typical for Cast 3xx.x Series Aluminium | |||
Temperatura de fusión | 546.0 - 621.0 °C Show Material materials with Temperatura de fusión of 546.0 - 621.0 °C | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 1.0 - 1.5 % Show Material materials with Cobre of 1.0 - 1.5 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Hierro | 0.60 % Show Material materials with Hierro of 0.60 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Magnesio | 0.4 - 0.6 % Show Material materials with Magnesio of 0.4 - 0.6 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Silicona | 4.5 - 5.5 % Show Material materials with Silicona of 4.5 - 5.5 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Titanio | 0.25 % Show Material materials with Titanio of 0.25 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Zinc | 0.35 % Show Material materials with Zinc of 0.35 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |