General
Property | Value | Comment |
---|---|---|
Densidad | 2.65 - 2.7 g/cm³ Show Material materials with Densidad of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 140.0 MPa Show Material materials with Bending Fatigue Strength of 140.0 MPa | F | Pink Sheets, ASTM B85 | Casting | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Módulo de cizallamiento | 2.8 GPa Show Material materials with Módulo de cizallamiento of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Módulo elástico | 73.0 - 80.0 GPa Show Material materials with Módulo elástico of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Resistencia a la tracción | 305.0 MPa Show Material materials with Resistencia a la tracción of 305.0 MPa | F | Pink Sheets, ASTM B85 | Casting |
Aplicaciones térmicas
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Calor específico | 960.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | |||
Coeficiente de dilatación térmica | 1.6e-05 - 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6e-05 - 2.3e-05 1/K | Typical for Cast 3xx.x Series Aluminium | |||
Conductividad térmica | 130.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 180.0 W/(m·K) | Typical for Cast 3xx.x Series Aluminium | |||
Temperatura de fusión | 557.0 - 596.0 °C Show Material materials with Temperatura de fusión of 557.0 - 596.0 °C | F | Pink Sheets, ASTM B85 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.6 % Show Material materials with Cobre of 0.6 % | F | Pink Sheets, ASTM B85 | Casting |
Estaño | 0.15 % Show Material materials with Estaño of 0.15 % | F | Pink Sheets, ASTM B85 | Casting |
Hierro | 2.00 % Show Material materials with Hierro of 2.00 % | F | Pink Sheets, ASTM B85 | Casting |
Magnesio | 0.4 - 0.6 % Show Material materials with Magnesio of 0.4 - 0.6 % | F | Pink Sheets, ASTM B85 | Casting |
Manganeso | 0.35 % Show Material materials with Manganeso of 0.35 % | F | Pink Sheets, ASTM B85 | Casting |
Níquel | 0.5 % Show Material materials with Níquel of 0.5 % | F | Pink Sheets, ASTM B85 | Casting |
Silicona | 9.0 - 10.0 % Show Material materials with Silicona of 9.0 - 10.0 % | F | Pink Sheets, ASTM B85 | Casting |
Zinc | 0.5 % Show Material materials with Zinc of 0.5 % | F | Pink Sheets, ASTM B85 | Casting |