General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.29 g/cm³ Show Supplier Material materials with Densidad of 1.29 g/cm³ | dry | ISO 1183 |
Índice límite de óxigeno | 35 % Show Supplier Material materials with Índice límite de óxigeno of 35 % | dry | ISO 4589-1/-2 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Módulo elástico | 3.8 GPa Show Supplier Material materials with Módulo elástico of 3.8 GPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 4.5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 4.5 kJ/m² | dry | ISO 179/1eA |
23 °C | 4.5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 4.5 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 40 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 40 kJ/m² | dry | ISO 179/1eU |
23 °C | 62 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 62 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure |
---|---|---|---|---|
Temperatura de flexión bajo carga | 175 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 175 °C | dry | ISO 75-1/-2 | 2 MPa |
Eléctrico
Property | Value | Condition | Frequency | Testing Standard |
---|---|---|---|---|
Constante dieléctrica | 2.6 [-] Show Supplier Material materials with Constante dieléctrica of 2.6 [-] | dry | 1MHz | IEC 60250 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Velocidad de flujo del volumen derretido | 35 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 35 cm³/10min | dry | ISO 1133 | 380°C/5kg |
Technological properties
Property | ||
---|---|---|
Application areas | Connectors,Fittings, Components, and Injection Molded Parts,Cable Ties,Chemical Process Industry,Chemical Process Industry - Coating of Chemical Pumps,Chemical Process Industry - Coating of Chemical Valves,Chemical Process Industry - Coating of Chemical Vessels,Chemical Process Industry - High Purity Piping,Chemical Process Industry - Injection Molding,Monofilaments,Powder Coatings - Wire Goods,Connectors E&E,Performance Wire,Wire and Cables,Natural Gas Distribution- Fittings | |
Processing methods | Injection Molding: |