General
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Absorción de agua | 0.03 % Show Supplier Material materials with Absorción de agua of 0.03 % | Sim. to ISO 62 | ||
0.03 - 0.05 % Show Supplier Material materials with Absorción de agua of 0.03 - 0.05 % | ASTM D570 | |||
Coefficient of friction | 0.19 [-] Show Supplier Material materials with Coefficient of friction of 0.19 [-] | ASTM D1894 | vs Steel, Kinetic | |
0.26 [-] Show Supplier Material materials with Coefficient of friction of 0.26 [-] | ASTM D1894 | vs Steel, Static | ||
Densidad | 1.77 - 1.8 g/cm³ Show Supplier Material materials with Densidad of 1.77 - 1.8 g/cm³ | ASTM D792 | ||
1.77 g/cm³ Show Supplier Material materials with Densidad of 1.77 g/cm³ | ISO 1183 | dry | ||
Moisture absorption | 0.015 % Show Supplier Material materials with Moisture absorption of 0.015 % | Sim. to ISO 62 | ||
Índice límite de óxigeno | 43 % Show Supplier Material materials with Índice límite de óxigeno of 43 % | ASTM D2863, ISO 4589-1/-2 | dry |
Mecánica
Property | Temperature | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|---|
Dureza Shore D | 70 - 75 [-] Show Supplier Material materials with Dureza Shore D of 70 - 75 [-] | ASTM D2240 | |||
Elongación | 30 - 200 % Show Supplier Material materials with Elongación of 30 - 200 % | ASTM D638 | |||
50 % Show Supplier Material materials with Elongación of 50 % | ISO 527-1/-2 | dry | min. | nominal | ||
Elongation at yield | 5 - 15 % Show Supplier Material materials with Elongation at yield of 5 - 15 % | ASTM D638 | |||
11 % Show Supplier Material materials with Elongation at yield of 11 % | ISO 527-1/-2 | dry | |||
Impact strength, Charpy notched, ASTM | 23 °C | 214 J/m Show Supplier Material materials with Impact strength, Charpy notched, ASTM of 214 J/m | ASTM D256 | min. | |
Impact strength, Charpy unnotched, ASTM | No Break at 23°C | ASTM D256 | |||
Límite elástico | 31 - 41.4 MPa Show Supplier Material materials with Límite elástico of 31 - 41.4 MPa | ASTM D638 | |||
40 MPa Show Supplier Material materials with Límite elástico of 40 MPa | ISO 527-1/-2 | dry | |||
Módulo de flexión | 1.0 - 1.2 GPa Show Supplier Material materials with Módulo de flexión of 1.0 - 1.2 GPa | ASTM D790 | |||
Módulo elástico | 1.0 - 1.5 GPa Show Supplier Material materials with Módulo elástico of 1.0 - 1.5 GPa | ASTM D638 | |||
1.3 GPa Show Supplier Material materials with Módulo elástico of 1.3 GPa | ISO 527-1/-2 | dry | |||
Resistencia a la compresión | 41.4 - 58.6 MPa Show Supplier Material materials with Resistencia a la compresión of 41.4 - 58.6 MPa | ASTM D695 | |||
Resistencia a la flexión | 20.7 - 34.5 MPa Show Supplier Material materials with Resistencia a la flexión of 20.7 - 34.5 MPa | ASTM D790 | at 5% strain | ||
Resistencia a la tracción | 27.6 - 48.3 MPa Show Supplier Material materials with Resistencia a la tracción of 27.6 - 48.3 MPa | ASTM D638 | |||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 5 kJ/m² | ISO 179/1eA | dry | No Break at 23°C |
Aplicaciones térmicas
Property | Value | Testing Standard | Condition | Pressure | Comment | ||||
---|---|---|---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 0.000126 - 0.000185 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.000126 - 0.000185 1/K | ASTM D696 | |||||||
0.00016 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.00016 1/K | ISO 11359-1/-2 | dry | |||||||
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | UL 746B | |||||||
Relative temperature index, mechanical strength | 140 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 140 °C | UL 746B | |||||||
Temperatura de flexión bajo carga | 38 - 55 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 38 - 55 °C | ASTM D648 | 2 MPa | 248 °F/hr | |||||
46 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 46 °C | ISO 75-1/-2 | dry | 2 MPa | ||||||
60 - 75 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 60 - 75 °C | ASTM D648 | 0.45 MPa | 248 °F/hr | ||||||
114 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 114 °C | ISO 75-1/-2 | dry | 0.45 MPa | ||||||
Temperatura de fusión | 155 - 160 °C Show Supplier Material materials with Temperatura de fusión of 155 - 160 °C | ASTM D3418 | |||||||
158 °C Show Supplier Material materials with Temperatura de fusión of 158 °C | ISO 11357-1/-3 | dry | 10°C/min | ||||||
Temperatura de reblandecimiento Vicat | 107 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 107 °C | ISO 306 | 50°C/h 50N | ||||||
Temperatura de transición del vidrio | -43 °C Show Supplier Material materials with Temperatura de transición del vidrio of -43 °C | ISO 11357-1/-2 | dry | 10°C/min | |||||
-40.6 - -38.3 °C Show Supplier Material materials with Temperatura de transición del vidrio of -40.6 - -38.3 °C | ASTM D7028 | ||||||||
Thermal decomposition in air | 375 °C Show Supplier Material materials with Thermal decomposition in air of 375 °C | TGA | 1% wt. loss | ||||||
Thermal decomposition in nitrogen | 410 °C Show Supplier Material materials with Thermal decomposition in nitrogen of 410 °C | TGA | 1% wt. loss | ||||||
Inflamabilidad | At thickness 1.5 mm IEC 60695-11-10: V-0, At thickness 0.8 mm IEC 60695-11-10: V-0 and yellow card available |
Eléctrico
Property | Value | Frequency | Testing Standard | Condition |
---|---|---|---|---|
Constante dieléctrica | 3.5 - 10.2 [-] Show Supplier Material materials with Constante dieléctrica of 3.5 - 10.2 [-] | 1KHz | ASTM D150 | |
6.5 [-] Show Supplier Material materials with Constante dieléctrica of 6.5 [-] | 1MHz | IEC 60250 | dry | |
10.5 [-] Show Supplier Material materials with Constante dieléctrica of 10.5 [-] | 100Hz | IEC 60250 | dry | |
Factor de disipación | 0.01 - 0.22 [-] Show Supplier Material materials with Factor de disipación of 0.01 - 0.22 [-] | 100KHz | ASTM D150 | |
0.038 [-] Show Supplier Material materials with Factor de disipación of 0.038 [-] | 100Hz | IEC 60250 | dry | |
0.234 [-] Show Supplier Material materials with Factor de disipación of 0.234 [-] | 1MHz | IEC 60250 | dry | |
Rigidez dieléctrica | 21 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 21 kV/mm | IEC 60243-1 | dry | |
51.2 - 63 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 51.2 - 63 kV/mm | ASTM D149 | |||
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | IEC 60093 | cond. | |
Volume resistivity | 2e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm | IEC 60093 | dry | |
2.9e+14 - 3.2e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2.9e+14 - 3.2e+14 Ω·cm | ASTM D257 | 65% RH | ||
Índice de seguimiento comparativo | 600 V Show Supplier Material materials with Índice de seguimiento comparativo of 600 V | IEC 60112 | dry |
Óptico
Property | Value | Testing Standard | Comment |
---|---|---|---|
Índice de refracción | 1 [-] Show Supplier Material materials with Índice de refracción of 1 [-] | ASTM D542 | sodium D line |
Rheological Properties
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Melt viscosity | 2300 - 2700 Pa·s Show Supplier Material materials with Melt viscosity of 2300 - 2700 Pa·s | ASTM D3835 | ||
Velocidad de flujo de la masa derretida | 3 - 8 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 3 - 8 g/10min | ASTM D1238 | 230°C/12.5kg | |
Velocidad de flujo del volumen derretido | 1.1 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 1.1 cm³/10min | ISO 1133 | dry | 230°C/5kg |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical Process Industry,Chemical Process Industry - High Purity Piping,Chemical Process Industry - Stock Shapes,Tubing and Hoses,Performance Wire,Plenum Cable,PVDF Cable Jacketing | |
Processing methods | Compression Molding: |