General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.78 g/cm³ Show Supplier Material materials with Densidad of 1.78 g/cm³ | dry | ISO 1183 |
Índice límite de óxigeno | 43 % Show Supplier Material materials with Índice límite de óxigeno of 43 % | dry | ISO 4589-1/-2 |
Mecánica
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Elongación | 50 % Show Supplier Material materials with Elongación of 50 % | dry | ISO 527-1/-2 | min. | nominal |
Elongation at yield | 10 % Show Supplier Material materials with Elongation at yield of 10 % | dry | ISO 527-1/-2 | |
Límite elástico | 35 MPa Show Supplier Material materials with Límite elástico of 35 MPa | dry | ISO 527-1/-2 | |
Módulo elástico | 1 GPa Show Supplier Material materials with Módulo elástico of 1 GPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | No Break at 23°C | dry | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment | ||||
---|---|---|---|---|---|---|---|---|---|
Temperatura de flexión bajo carga | 84 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 84 °C | dry | ISO 75-1/-2 | 2 MPa | |||||
Temperatura de fusión | 165 °C Show Supplier Material materials with Temperatura de fusión of 165 °C | dry | ISO 11357-1/-3 | 10°C/min | |||||
Temperatura de transición del vidrio | -40 °C Show Supplier Material materials with Temperatura de transición del vidrio of -40 °C | dry | ISO 11357-1/-2 | 10°C/min | |||||
Inflamabilidad | At thickness 1.5 mm IEC 60695-11-10: V-0 and yellow card available |
Eléctrico
Property | Value | Condition | Testing Standard |
---|---|---|---|
Surface resistivity | 10000 Ω/sq Show Supplier Material materials with Surface resistivity of 10000 Ω/sq | cond. | IEC 60093 |
Volume resistivity | 1e+06 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+06 Ω·cm | dry | IEC 60093 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Velocidad de flujo del volumen derretido | 8 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 8 cm³/10min | dry | ISO 1133 | 230°C/10kg |
Technological properties
Property | ||
---|---|---|
Application areas | Fittings, Components, and Injection Molded Parts,Fuel Management - Fuel Lines,Fuel Management - In-Tank and Fuel Venting Lines,Chemical Process Industry,Permanent Antistatic Solutions,Tubing and Hoses | |
Processing methods | Injection Molding: |