General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Densidad | 1.78 g/cm³ Show Supplier Material materials with Densidad of 1.78 g/cm³ | dry | ISO 1183 |
1.84 - 1.88 g/cm³ Show Supplier Material materials with Densidad of 1.84 - 1.88 g/cm³ | ASTM D792 | ||
Índice límite de óxigeno | 43 % Show Supplier Material materials with Índice límite de óxigeno of 43 % | dry | ISO 4589-1/-2 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elongación | 40 % Show Supplier Material materials with Elongación of 40 % | dry | ISO 527-1/-2 | min. | nominal | |
Elongation at yield | 5 % Show Supplier Material materials with Elongation at yield of 5 % | dry | ISO 527-1/-2 | ||
Límite elástico | 45 MPa Show Supplier Material materials with Límite elástico of 45 MPa | dry | ISO 527-1/-2 | ||
Módulo elástico | 1.6 GPa Show Supplier Material materials with Módulo elástico of 1.6 GPa | dry | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | dry | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Temperatura de fusión | 165 - 172 °C Show Supplier Material materials with Temperatura de fusión of 165 - 172 °C | ASTM D3418 | ||
166 °C Show Supplier Material materials with Temperatura de fusión of 166 °C | ISO 11357-1/-3 | dry | 10°C/min |
Eléctrico
Property | Value | Condition | Frequency | Testing Standard |
---|---|---|---|---|
Constante dieléctrica | 0.07 [-] Show Supplier Material materials with Constante dieléctrica of 0.07 [-] | dry | 100Hz | IEC 60250 |
Rigidez dieléctrica | 27 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 27 kV/mm | dry | IEC 60243-1 | |
Surface resistivity | 10000 Ω/sq Show Supplier Material materials with Surface resistivity of 10000 Ω/sq | cond. | IEC 60093 | |
Volume resistivity | 1e+06 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+06 Ω·cm | dry | IEC 60093 |
Rheological Properties
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Melt viscosity | 2500 Pa·s Show Supplier Material materials with Melt viscosity of 2500 Pa·s | ASTM D3835 | ||
Velocidad de flujo de la masa derretida | 3 - 8 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 3 - 8 g/10min | ASTM D1238 | 230°C/10kg | |
Velocidad de flujo del volumen derretido | 4 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 4 cm³/10min | ISO 1133 | dry | 230°C/10kg |
Technological properties
Property | ||
---|---|---|
Application areas | Fuel Management - In-Tank and Fuel Venting Lines,Chemical Process Industry,Chemical Process Industry - Stock Shapes,Permanent Antistatic Solutions | |
Fillers | Carbon Black |