General
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Absorción de agua | 0.04 % Show Supplier Material materials with Absorción de agua of 0.04 % | Sim. to ISO 62, ASTM D570 | max. | |
Coefficient of friction | 0.17 [-] Show Supplier Material materials with Coefficient of friction of 0.17 [-] | ASTM D1894 | vs Steel, Kinetic | |
0.23 [-] Show Supplier Material materials with Coefficient of friction of 0.23 [-] | ASTM D1894 | vs Steel, Static | ||
Densidad | 1.75 - 1.77 g/cm³ Show Supplier Material materials with Densidad of 1.75 - 1.77 g/cm³ | ASTM D792 | ||
1.76 g/cm³ Show Supplier Material materials with Densidad of 1.76 g/cm³ | ISO 1183 | dry | ||
Índice límite de óxigeno | 43 % Show Supplier Material materials with Índice límite de óxigeno of 43 % | ISO 4589-1/-2 | dry | |
44 % Show Supplier Material materials with Índice límite de óxigeno of 44 % | ASTM D2863 |
Mecánica
Property | Temperature | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|---|
Dureza Shore D | 75 - 80 [-] Show Supplier Material materials with Dureza Shore D of 75 - 80 [-] | ASTM D2240 | |||
Elongación | 50 - 250 % Show Supplier Material materials with Elongación of 50 - 250 % | ASTM D638 | |||
50 % Show Supplier Material materials with Elongación of 50 % | ISO 527-1/-2 | dry | min. | nominal | ||
Elongation at yield | 10 - 15 % Show Supplier Material materials with Elongation at yield of 10 - 15 % | ASTM D638 | |||
13 % Show Supplier Material materials with Elongation at yield of 13 % | ISO 527-1/-2 | dry | |||
Impact strength, Charpy notched, ASTM | 23 °C | 96.1 - 214 J/m Show Supplier Material materials with Impact strength, Charpy notched, ASTM of 96.1 - 214 J/m | ASTM D256 | ||
Impact strength, Charpy unnotched, ASTM | 23 °C | 801 - 2140 J/m Show Supplier Material materials with Impact strength, Charpy unnotched, ASTM of 801 - 2140 J/m | ASTM D256 | ||
Límite elástico | 34.5 - 51.7 MPa Show Supplier Material materials with Límite elástico of 34.5 - 51.7 MPa | ASTM D638 | |||
52 MPa Show Supplier Material materials with Límite elástico of 52 MPa | ISO 527-1/-2 | dry | |||
Módulo de flexión | 1.4 - 1.8 GPa Show Supplier Material materials with Módulo de flexión of 1.4 - 1.8 GPa | ASTM D790 | |||
Módulo elástico | 1.0 - 1.4 GPa Show Supplier Material materials with Módulo elástico of 1.0 - 1.4 GPa | ASTM D638 | |||
1.4 GPa Show Supplier Material materials with Módulo elástico of 1.4 GPa | ISO 527-1/-2 | dry | |||
Resistencia a la compresión | 55.2 - 68.9 MPa Show Supplier Material materials with Resistencia a la compresión of 55.2 - 68.9 MPa | ASTM D695 | |||
Resistencia a la flexión | 48.3 - 62.1 MPa Show Supplier Material materials with Resistencia a la flexión of 48.3 - 62.1 MPa | ASTM D790 | at 5% strain | ||
Resistencia a la tracción | 31 - 48.3 MPa Show Supplier Material materials with Resistencia a la tracción of 31 - 48.3 MPa | ASTM D638 |
Aplicaciones térmicas
Property | Value | Testing Standard | Pressure | Condition | Comment | ||||
---|---|---|---|---|---|---|---|---|---|
Calor específico | 745 - 958 J/(kg·K) Show Supplier Material materials with Calor específico of 745 - 958 J/(kg·K) | DSC | |||||||
Coeficiente de dilatación térmica | 9e-05 - 0.000126 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 9e-05 - 0.000126 1/K | ASTM D696 | |||||||
Conductividad térmica | 0.17 - 0.19 W/(m·K) Show Supplier Material materials with Conductividad térmica of 0.17 - 0.19 W/(m·K) | ASTM D433 | |||||||
Temperatura de flexión bajo carga | 80 - 90 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 80 - 90 °C | ASTM D648 | 2 MPa | 248 °F/hr | |||||
85 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 85 °C | ISO 75-1/-2 | 2 MPa | dry | ||||||
112 - 140 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 112 - 140 °C | ASTM D648 | 0.45 MPa | 248 °F/hr | ||||||
Temperatura de fusión | 155 - 172 °C Show Supplier Material materials with Temperatura de fusión of 155 - 172 °C | ASTM D3418 | |||||||
161 °C Show Supplier Material materials with Temperatura de fusión of 161 °C | ISO 11357-1/-3 | dry | 10°C/min | ||||||
Temperatura de transición del vidrio | -40.6 - -38.3 °C Show Supplier Material materials with Temperatura de transición del vidrio of -40.6 - -38.3 °C | ASTM D7028 | |||||||
-40 °C Show Supplier Material materials with Temperatura de transición del vidrio of -40 °C | ISO 11357-1/-2 | dry | 10°C/min | ||||||
Thermal decomposition in air | 375 °C Show Supplier Material materials with Thermal decomposition in air of 375 °C | TGA | 1% wt. loss | ||||||
Thermal decomposition in nitrogen | 410 °C Show Supplier Material materials with Thermal decomposition in nitrogen of 410 °C | TGA | 1% wt. loss | ||||||
Inflamabilidad | At thickness 1.6 mm IEC 60695-11-10: V-0, At thickness 0.8 mm IEC 60695-11-10: V-0 |
Eléctrico
Property | Value | Frequency | Testing Standard | Condition |
---|---|---|---|---|
Constante dieléctrica | 4.5 - 9.5 [-] Show Supplier Material materials with Constante dieléctrica of 4.5 - 9.5 [-] | 1KHz | ASTM D150 | |
6.7 [-] Show Supplier Material materials with Constante dieléctrica of 6.7 [-] | 1MHz | IEC 60250 | dry | |
9 [-] Show Supplier Material materials with Constante dieléctrica of 9 [-] | 100Hz | IEC 60250 | dry | |
Factor de disipación | 0.01 - 0.21 [-] Show Supplier Material materials with Factor de disipación of 0.01 - 0.21 [-] | 100KHz | ASTM D150 | |
0.07 [-] Show Supplier Material materials with Factor de disipación of 0.07 [-] | 1MHz | IEC 60250 | dry | |
0.13 [-] Show Supplier Material materials with Factor de disipación of 0.13 [-] | 100Hz | IEC 60250 | dry | |
Rigidez dieléctrica | 63 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 63 kV/mm | ASTM D149, IEC 60243-1 | dry | |
Surface resistivity | 5.1e+11 - 5.3e+11 Ω/sq Show Supplier Material materials with Surface resistivity of 5.1e+11 - 5.3e+11 Ω/sq | ASTM D257 | ||
Volume resistivity | 2e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm | ASTM D257 | 65% RH | |
2e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm | IEC 60093 | dry |
Óptico
Property | Value | Testing Standard | Comment |
---|---|---|---|
Índice de refracción | 1 [-] Show Supplier Material materials with Índice de refracción of 1 [-] | ASTM D542 | sodium D line |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 2 % Show Supplier Material materials with Contracción of 2 % | dry | ISO 294-4 | |
2 % Show Supplier Material materials with Contracción of 2 % | dry | ISO 294-4 | Transverse | |
Melt viscosity | 2350 - 2950 Pa·s Show Supplier Material materials with Melt viscosity of 2350 - 2950 Pa·s | ASTM D3835 | ||
Thermal conductivity of melt | 0.19 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.19 W/(m·K) | |||
Velocidad de flujo de la masa derretida | 6 - 14 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 6 - 14 g/10min | ASTM D1238 | 230°C/21.6kg | |
Velocidad de flujo del volumen derretido | 5.6 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 5.6 cm³/10min | dry | ISO 1133 | 230°C/21.6kg |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical Process Industry,Chemical Process Industry - Injection Molding,Chemical Process Industry - Stock Shapes,Monofilaments,Tower Packing,Automotive Cables,Performance Wire,Plenum Cable,PVDF Cable Jacketing,Wire and Cables |