General
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Absorción de agua | 0.01 - 0.03 % Show Supplier Material materials with Absorción de agua of 0.01 - 0.03 % | ASTM D570 | ||
0.03 % Show Supplier Material materials with Absorción de agua of 0.03 % | Sim. to ISO 62 | |||
Coefficient of friction | 0.14 [-] Show Supplier Material materials with Coefficient of friction of 0.14 [-] | ASTM D1894 | vs Steel, Kinetic | |
0.2 [-] Show Supplier Material materials with Coefficient of friction of 0.2 [-] | ASTM D1894 | vs Steel, Static | ||
Densidad | 1.76 - 1.78 g/cm³ Show Supplier Material materials with Densidad of 1.76 - 1.78 g/cm³ | ASTM D792 | ||
Moisture absorption | 0.015 % Show Supplier Material materials with Moisture absorption of 0.015 % | Sim. to ISO 62 | ||
Índice límite de óxigeno | 60 % Show Supplier Material materials with Índice límite de óxigeno of 60 % | ASTM D2863 | ||
67 % Show Supplier Material materials with Índice límite de óxigeno of 67 % | ISO 4589-1/-2 | dry |
Mecánica
Property | Temperature | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|---|
Dureza Shore D | 76 - 80 [-] Show Supplier Material materials with Dureza Shore D of 76 - 80 [-] | ASTM D2240 | |||
Elongación | 20 - 100 % Show Supplier Material materials with Elongación of 20 - 100 % | ASTM D638 | |||
40 % Show Supplier Material materials with Elongación of 40 % | ISO 527-1/-2 | dry | min. | nominal | ||
Elongation at yield | 5 - 10 % Show Supplier Material materials with Elongation at yield of 5 - 10 % | ASTM D638 | |||
8 % Show Supplier Material materials with Elongation at yield of 8 % | ISO 527-1/-2 | dry | |||
Impact strength, Charpy notched, ASTM | 23 °C | 96.1 - 214 J/m Show Supplier Material materials with Impact strength, Charpy notched, ASTM of 96.1 - 214 J/m | ASTM D256 | ||
Impact strength, Charpy unnotched, ASTM | 23 °C | 1070 - 4270 J/m Show Supplier Material materials with Impact strength, Charpy unnotched, ASTM of 1070 - 4270 J/m | ASTM D256 | ||
Límite elástico | 44.8 - 55.2 MPa Show Supplier Material materials with Límite elástico of 44.8 - 55.2 MPa | ASTM D638 | |||
54 MPa Show Supplier Material materials with Límite elástico of 54 MPa | ISO 527-1/-2 | dry | |||
Módulo de flexión | 1.4 - 2.3 GPa Show Supplier Material materials with Módulo de flexión of 1.4 - 2.3 GPa | ASTM D790 | |||
Módulo elástico | 1.4 - 2.3 GPa Show Supplier Material materials with Módulo elástico of 1.4 - 2.3 GPa | ASTM D638 | |||
2.5 GPa Show Supplier Material materials with Módulo elástico of 2.5 GPa | ISO 527-1/-2 | dry | |||
Resistencia a la compresión | 68.9 - 103 MPa Show Supplier Material materials with Resistencia a la compresión of 68.9 - 103 MPa | ASTM D695 | |||
Resistencia a la flexión | 58.6 - 75.8 MPa Show Supplier Material materials with Resistencia a la flexión of 58.6 - 75.8 MPa | ASTM D790 | at 5% strain | ||
Resistencia a la tracción | 34.5 - 55.2 MPa Show Supplier Material materials with Resistencia a la tracción of 34.5 - 55.2 MPa | ASTM D638 | |||
Resistencia al choque, ensayo Charpy entallado | -30 °C | 5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 5 kJ/m² | ISO 179/1eA | dry | |
23 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | ISO 179/1eA | dry | ||
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 218 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 218 kJ/m² | ISO 179/1eU | dry | |
23 °C | 232 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 232 kJ/m² | ISO 179/1eU | dry |
Aplicaciones térmicas
Property | Value | Testing Standard | Condition | Pressure | Comment | ||||
---|---|---|---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 0.000119 - 0.000144 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.000119 - 0.000144 1/K | ASTM D696 | |||||||
0.000136 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.000136 1/K | ISO 11359-1/-2 | dry | |||||||
Temperatura de flexión bajo carga | 105 - 115 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 105 - 115 °C | ASTM D648 | 2 MPa | 248 °F/hr | |||||
110 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 110 °C | ISO 75-1/-2 | dry | 2 MPa | ||||||
125 - 140 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 125 - 140 °C | ASTM D648 | 0.45 MPa | 248 °F/hr | ||||||
Temperatura de fusión | 165 - 172 °C Show Supplier Material materials with Temperatura de fusión of 165 - 172 °C | ASTM D3418 | |||||||
171 °C Show Supplier Material materials with Temperatura de fusión of 171 °C | ISO 11357-1/-3 | dry | 10°C/min | ||||||
Temperatura de reblandecimiento Vicat | 141 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 141 °C | ISO 306 | 50°C/h 50N | ||||||
Temperatura de transición del vidrio | -40.6 - -38.3 °C Show Supplier Material materials with Temperatura de transición del vidrio of -40.6 - -38.3 °C | ASTM D7028 | |||||||
-40 °C Show Supplier Material materials with Temperatura de transición del vidrio of -40 °C | ISO 11357-1/-2 | dry | 10°C/min | ||||||
Thermal decomposition in air | 375 °C Show Supplier Material materials with Thermal decomposition in air of 375 °C | TGA | 1% wt. loss | ||||||
Thermal decomposition in nitrogen | 410 °C Show Supplier Material materials with Thermal decomposition in nitrogen of 410 °C | TGA | 1% wt. loss | ||||||
Inflamabilidad | At thickness 1.6 mm IEC 60695-11-10: V-0, At thickness 0.8 mm IEC 60695-11-10: V-0 |
Eléctrico
Property | Value | Frequency | Testing Standard | Condition |
---|---|---|---|---|
Constante dieléctrica | 4.5 - 9.5 [-] Show Supplier Material materials with Constante dieléctrica of 4.5 - 9.5 [-] | 1KHz | ASTM D150 | |
7.5 [-] Show Supplier Material materials with Constante dieléctrica of 7.5 [-] | 1MHz | IEC 60250 | dry | |
10 [-] Show Supplier Material materials with Constante dieléctrica of 10 [-] | 100Hz | IEC 60250 | dry | |
Factor de disipación | 0.01 - 0.21 [-] Show Supplier Material materials with Factor de disipación of 0.01 - 0.21 [-] | 100KHz | ASTM D150 | |
0.031 [-] Show Supplier Material materials with Factor de disipación of 0.031 [-] | 100Hz | IEC 60250 | dry | |
0.216 [-] Show Supplier Material materials with Factor de disipación of 0.216 [-] | 1MHz | IEC 60250 | dry | |
Rigidez dieléctrica | 67 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 67 kV/mm | ASTM D149 | ||
Volume resistivity | 2e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm | ASTM D257 | 65% RH |
Óptico
Property | Value | Testing Standard | Comment |
---|---|---|---|
Índice de refracción | 1 [-] Show Supplier Material materials with Índice de refracción of 1 [-] | ASTM D542 | sodium D line |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 2 % Show Supplier Material materials with Contracción of 2 % | dry | ISO 294-4 | |
2 % Show Supplier Material materials with Contracción of 2 % | dry | ISO 294-4 | Transverse | |
Melt viscosity | 500 - 800 Pa·s Show Supplier Material materials with Melt viscosity of 500 - 800 Pa·s | ASTM D3835 | ||
Velocidad de flujo de la masa derretida | 16 - 30 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 16 - 30 g/10min | ASTM D1238 | 230°C/5kg | |
Velocidad de flujo del volumen derretido | 10 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 10 cm³/10min | dry | ISO 1133 | 230°C/5kg |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical Process Industry,Chemical Process Industry - Injection Molding | |
Processing methods | Injection Molding: |