Medidas
Property | Value |
---|---|
Ancho | 900 mm Show Supplier Material materials with Ancho of 900 mm |
Espesor | 255 - 355 mm Show Supplier Material materials with Espesor of 255 - 355 mm |
Mecánica
Property | Value | Comment |
---|---|---|
Dureza Brinell | 230 [-] Show Supplier Material materials with Dureza Brinell of 230 [-] | soft annealed |
Dureza Rockwell C | 40 - 56 [-] Show Supplier Material materials with Dureza Rockwell C of 40 - 56 [-] | |
Resistencia a la tracción | 1555 - 1775 MPa Show Supplier Material materials with Resistencia a la tracción of 1555 - 1775 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 100 °C | 1.07e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.07e-05 1/K | for 20°C to the mentioned temperature |
150 °C | 1.1e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.1e-05 1/K | for 20°C to the mentioned temperature | |
200 °C | 1.12e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.12e-05 1/K | for 20°C to the mentioned temperature | |
250 °C | 1.15e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.15e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.17e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.17e-05 1/K | for 20°C to the mentioned temperature | |
350 °C | 1.19e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.21e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.21e-05 1/K | for 20°C to the mentioned temperature | |
450 °C | 1.23e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.23e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.24e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.24e-05 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 23 °C | 21.5 W/(m·K) Show Supplier Material materials with Conductividad térmica of 21.5 W/(m·K) | |
150 °C | 23.2 W/(m·K) Show Supplier Material materials with Conductividad térmica of 23.2 W/(m·K) | ||
300 °C | 23.9 W/(m·K) Show Supplier Material materials with Conductividad térmica of 23.9 W/(m·K) | ||
350 °C | 24.3 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.3 W/(m·K) | ||
400 °C | 24.2 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.2 W/(m·K) | ||
500 °C | 24 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbono | 0.37 % Show Supplier Material materials with Carbono of 0.37 % |
Cromo | 13.6 % Show Supplier Material materials with Cromo of 13.6 % |
Hierro | Balance |
Manganeso | 0.5 % Show Supplier Material materials with Manganeso of 0.5 % |
Silicona | 0.9 % Show Supplier Material materials with Silicona of 0.9 % |
Vanadio | 0.3 % Show Supplier Material materials with Vanadio of 0.3 % |
Technological properties
Property | ||
---|---|---|
Application areas | Moulds and inserts for processing corrosive acting plastics. | |
Heat Treatment | Soft annealing: 760-800°C (Cooling in furnace) - Hardening: 1000-1050°C and quenching in air, oil or hot bath T=500-550°C |