General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8.3 g/cm³ Show Material materials with Densidad of 8.3 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Rockwell B | 23.0 °C | 80 [-] Show Material materials with Dureza Rockwell B of 80 [-] | |
Elongación | 23.0 °C | 35 % Show Material materials with Elongación of 35 % | in 2 in. |
Límite elástico | 23.0 °C | 276 MPa Show Material materials with Límite elástico of 276 MPa | |
Módulo elástico | 23.0 °C | 159 GPa Show Material materials with Módulo elástico of 159 GPa | |
Resistencia a la tracción | 23.0 °C | 552 MPa Show Material materials with Resistencia a la tracción of 552 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 502 J/(kg·K) Show Material materials with Calor específico of 502 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | from 30°C to the mentioned temperature |
150.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | from 30°C to the mentioned temperature | |
200.0 °C | 1.04E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
250.0 °C | 1.04E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
300.0 °C | 1.02E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 1/K | from 30°C to the mentioned temperature | |
350.0 °C | 1.02E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 1/K | from 30°C to the mentioned temperature | |
400.0 °C | 1.01E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.01E-5 1/K | from 30°C to the mentioned temperature | |
450.0 °C | 1.07E-5 - 9.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.07E-5 - 9.6E-5 1/K | from 30°C to the mentioned temperature | |
475.0 °C | 1.01E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.01E-5 1/K | from 30°C to the mentioned temperature | |
500.0 °C | 1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 1/K | from 30°C to the mentioned temperature | |
525.0 °C | 1.04E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
550.0 °C | 1.02E-5 - 1.07E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 - 1.07E-5 1/K | from 30°C to the mentioned temperature | |
600.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | from 30°C to the mentioned temperature | |
700.0 °C | 1.17E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.17E-5 1/K | from 30°C to the mentioned temperature | |
800.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | from 30°C to the mentioned temperature | |
900.0 °C | 1.33E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.33E-5 1/K | from 30°C to the mentioned temperature | |
1009.0 °C | 1.42E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.42E-5 1/K | from 30°C to the mentioned temperature | |
Conductividad térmica | 23.0 °C | 14 W/(m·K) Show Material materials with Conductividad térmica of 14 W/(m·K) | |
Temperatura de fusión | 1427 °C Show Material materials with Temperatura de fusión of 1427 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 23.0 °C | 4.4E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.4E-7 Ω·m |
Magnético
Property | Value |
---|---|
Temperatura de Curie | 530 °C Show Material materials with Temperatura de Curie of 530 °C |
Chemical properties
Property | Value |
---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % |
Carbono | 0.05 % Show Material materials with Carbono of 0.05 % |
Cromo | 0.03 % Show Material materials with Cromo of 0.03 % |
Hierro | Balance |
Níquel | 50.5 % Show Material materials with Níquel of 50.5 % |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % |
Technological properties
Property | ||
---|---|---|
Application areas | Common applications of Alloy 52: Pin feed-throughs for semiconductor devices, glass-to-metal sealing with soft glass for mercury switches and semiconductor devices |