General
Property | Temperature | Value | Related Standards |
---|---|---|---|
Densidad | 20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | EN 573-3 |
Mecánica
Property | Temperature | Value | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | EN 573-3 | |
Elongación | -196.0 °C | 23.0 - 30.0 % Show Material materials with Elongación of 23.0 - 30.0 % | EN 573-3 | |
-196.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | EN 573-3 | ||
-196.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | EN 573-3 | ||
-80.0 °C | 11.0 - 18.0 % Show Material materials with Elongación of 11.0 - 18.0 % | EN 573-3 | ||
-80.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | EN 573-3 | ||
-80.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | EN 573-3 | ||
-28.0 °C | 10.0 - 16.0 % Show Material materials with Elongación of 10.0 - 16.0 % | EN 573-3 | ||
-28.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | EN 573-3 | ||
-28.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | EN 573-3 | ||
20.0 °C | 10.0 - 16.0 % Show Material materials with Elongación of 10.0 - 16.0 % | EN 573-3 | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | EN 573-3 | ||
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | EN 573-3 | ||
100.0 °C | 10.0 - 16.0 % Show Material materials with Elongación of 10.0 - 16.0 % | EN 573-3 | ||
100.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | EN 573-3 | ||
100.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | EN 573-3 | ||
150.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | EN 573-3 | ||
150.0 °C | 11.0 - 16.0 % Show Material materials with Elongación of 11.0 - 16.0 % | EN 573-3 | ||
150.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | EN 573-3 | ||
200.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | EN 573-3 | ||
200.0 °C | 18.0 - 20.0 % Show Material materials with Elongación of 18.0 - 20.0 % | EN 573-3 | ||
200.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | EN 573-3 | ||
260.0 °C | 60.0 % Show Material materials with Elongación of 60.0 % | EN 573-3 | ||
315.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | EN 573-3 | ||
370.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | EN 573-3 | ||
Límite elástico | -196.0 °C | 170.0 MPa Show Material materials with Límite elástico of 170.0 MPa | EN 573-3 | RP02 |
-196.0 °C | 170.0 - 230.0 MPa Show Material materials with Límite elástico of 170.0 - 230.0 MPa | EN 573-3 | RP02 | |
-196.0 °C | 230.0 MPa Show Material materials with Límite elástico of 230.0 MPa | EN 573-3 | RP02 | |
-80.0 °C | 150.0 MPa Show Material materials with Límite elástico of 150.0 MPa | EN 573-3 | RP02 | |
-80.0 °C | 150.0 - 200.0 MPa Show Material materials with Límite elástico of 150.0 - 200.0 MPa | EN 573-3 | RP02 | |
-80.0 °C | 200.0 MPa Show Material materials with Límite elástico of 200.0 MPa | EN 573-3 | RP02 | |
-28.0 °C | 140.0 MPa Show Material materials with Límite elástico of 140.0 MPa | EN 573-3 | RP02 | |
-28.0 °C | 140.0 - 190.0 MPa Show Material materials with Límite elástico of 140.0 - 190.0 MPa | EN 573-3 | RP02 | |
-28.0 °C | 190.0 MPa Show Material materials with Límite elástico of 190.0 MPa | EN 573-3 | RP02 | |
57.0 MPa Show Material materials with Límite elástico of 57.0 MPa | ||||
20.0 °C | 140.0 MPa Show Material materials with Límite elástico of 140.0 MPa | EN 573-3 | RP02 | |
20.0 °C | 140.0 - 185.0 MPa Show Material materials with Límite elástico of 140.0 - 185.0 MPa | EN 573-3 | RP02 | |
20.0 °C | 185.0 MPa Show Material materials with Límite elástico of 185.0 MPa | EN 573-3 | RP02 | |
100.0 °C | 130.0 MPa Show Material materials with Límite elástico of 130.0 MPa | EN 573-3 | RP02 | |
100.0 °C | 130.0 - 145.0 MPa Show Material materials with Límite elástico of 130.0 - 145.0 MPa | EN 573-3 | RP02 | |
100.0 °C | 145.0 MPa Show Material materials with Límite elástico of 145.0 MPa | EN 573-3 | RP02 | |
150.0 °C | 110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | EN 573-3 | RP02 | |
200.0 °C | 60.0 MPa Show Material materials with Límite elástico of 60.0 MPa | EN 573-3 | RP02 | |
260.0 °C | 30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | EN 573-3 | RP02 | |
315.0 °C | 15.0 MPa Show Material materials with Límite elástico of 15.0 MPa | EN 573-3 | RP02 | |
370.0 °C | 10.0 MPa Show Material materials with Límite elástico of 10.0 MPa | EN 573-3 | RP02 | |
Módulo de cizallamiento | 20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | EN 573-3 | |
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.1 GPa | EN 573-3 | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.1 - 26.5 GPa | EN 573-3 | ||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | EN 573-3 | ||
Módulo elástico | -270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | EN 573-3 | |
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Módulo elástico of 60.0 - 70.0 GPa | EN 573-3 | ||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | EN 573-3 | ||
20.0 °C | 60.0 - 69.5 GPa Show Material materials with Módulo elástico of 60.0 - 69.5 GPa | EN 573-3 | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Módulo elástico of 60.0 - 69.0 GPa | EN 573-3 | ||
20.0 °C | 65.0 - 70.0 GPa Show Material materials with Módulo elástico of 65.0 - 70.0 GPa | EN 573-3 | ||
20.0 °C | 65.0 - 69.5 GPa Show Material materials with Módulo elástico of 65.0 - 69.5 GPa | EN 573-3 | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Módulo elástico of 65.0 - 69.0 GPa | EN 573-3 | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | EN 573-3 | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | EN 573-3 | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Módulo elástico of 69.0 - 69.5 GPa | EN 573-3 | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Módulo elástico of 69.5 - 70.0 GPa | EN 573-3 | ||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | EN 573-3 | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | EN 573-3 | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | EN 573-3 | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | EN 573-3 | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | EN 573-3 | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | EN 573-3 | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | EN 573-3 | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | EN 573-3 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Resistencia a la tracción | -196.0 °C | 240.0 MPa Show Material materials with Resistencia a la tracción of 240.0 MPa | EN 573-3 | |
-196.0 °C | 240.0 - 280.0 MPa Show Material materials with Resistencia a la tracción of 240.0 - 280.0 MPa | EN 573-3 | ||
-196.0 °C | 280.0 MPa Show Material materials with Resistencia a la tracción of 280.0 MPa | EN 573-3 | ||
-80.0 °C | 165.0 MPa Show Material materials with Resistencia a la tracción of 165.0 MPa | EN 573-3 | ||
-80.0 °C | 165.0 - 220.0 MPa Show Material materials with Resistencia a la tracción of 165.0 - 220.0 MPa | EN 573-3 | ||
-80.0 °C | 220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | EN 573-3 | ||
-28.0 °C | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | EN 573-3 | ||
-28.0 °C | 150.0 - 205.0 MPa Show Material materials with Resistencia a la tracción of 150.0 - 205.0 MPa | EN 573-3 | ||
-28.0 °C | 205.0 MPa Show Material materials with Resistencia a la tracción of 205.0 MPa | EN 573-3 | ||
128.0 MPa Show Material materials with Resistencia a la tracción of 128.0 MPa | ||||
20.0 °C | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | EN 573-3 | ||
20.0 °C | 150.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 150.0 - 200.0 MPa | EN 573-3 | ||
20.0 °C | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | EN 573-3 | ||
100.0 °C | 145.0 MPa Show Material materials with Resistencia a la tracción of 145.0 MPa | EN 573-3 | ||
100.0 °C | 145.0 - 180.0 MPa Show Material materials with Resistencia a la tracción of 145.0 - 180.0 MPa | EN 573-3 | ||
100.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | EN 573-3 | ||
150.0 °C | 125.0 MPa Show Material materials with Resistencia a la tracción of 125.0 MPa | EN 573-3 | ||
150.0 °C | 125.0 - 160.0 MPa Show Material materials with Resistencia a la tracción of 125.0 - 160.0 MPa | EN 573-3 | ||
150.0 °C | 160.0 MPa Show Material materials with Resistencia a la tracción of 160.0 MPa | EN 573-3 | ||
200.0 °C | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | EN 573-3 | ||
260.0 °C | 50.0 MPa Show Material materials with Resistencia a la tracción of 50.0 MPa | EN 573-3 | ||
315.0 °C | 30.0 MPa Show Material materials with Resistencia a la tracción of 30.0 MPa | EN 573-3 | ||
370.0 °C | 20.0 MPa Show Material materials with Resistencia a la tracción of 20.0 MPa | EN 573-3 |
Aplicaciones térmicas
Property | Temperature | Value | Related Standards | Comment |
---|---|---|---|---|
Calor específico | 20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Calor específico of 892.0 - 893.0 J/(kg·K) | EN 573-3 | |
20.0 °C | 892.0 J/(kg·K) Show Material materials with Calor específico of 892.0 J/(kg·K) | EN 573-3 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | EN 573-3 | ||
Coeficiente de dilatación térmica | -50.0 °C | 2.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.15e-05 1/K | EN 573-3 | |
2.33e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.33e-05 1/K | ||||
100.0 °C | 2.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.32e-05 1/K | EN 573-3 | ||
200.0 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | EN 573-3 | ||
300.0 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | EN 573-3 | ||
Conductividad térmica | 175.0 W/(m·K) Show Material materials with Conductividad térmica of 175.0 W/(m·K) | |||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | EN 573-3 | ||
20.0 °C | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | EN 573-3 | ||
Temperatura de fusión | 629.0 - 654.0 °C Show Material materials with Temperatura de fusión of 629.0 - 654.0 °C | Typical for Wrought 3000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Related Standards |
---|---|---|---|
Conductividad eléctrica | 20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 29000000.0 S/m | EN 573-3 |
20.0 °C | 23000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 29000000.0 S/m | EN 573-3 | |
Resistividad eléctrica | 20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.1e-08 Ω·m | EN 573-3 |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.5e-08 Ω·m | EN 573-3 | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 Ω·m | EN 573-3 | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 - 4.5e-08 Ω·m | EN 573-3 |
Chemical properties
Property | Value | Related Standards |
---|---|---|
Cobre | 0.05 - 0.2 % Show Material materials with Cobre of 0.05 - 0.2 % | EN 573-3 |
Hierro | 0.7 Show Material materials with Hierro of 0.7 | EN 573-3 |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | EN 573-3 |
Silicona | 0.6 Show Material materials with Silicona of 0.6 | EN 573-3 |
Zinc | 0.1 Show Material materials with Zinc of 0.1 | EN 573-3 |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |