General
Property | Value | Comment |
---|---|---|
Densidad | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | ||||
Dureza Brinell | 260 [-] Show Material materials with Dureza Brinell of 260 [-] | Predicted Value, Transverse | ||||
Elongación | 9.6 % Show Material materials with Elongación of 9.6 % | Predicted Value, A80 | ||||
10.3 % Show Material materials with Elongación of 10.3 % | Predicted Value, A200 | |||||
10.6 % Show Material materials with Elongación of 10.6 % | Predicted Value, Transverse | |||||
11.2 % Show Material materials with Elongación of 11.2 % | Predicted Value, A50 | |||||
16.1 % Show Material materials with Elongación of 16.1 % | Predicted Value, A5 | |||||
19.3 % Show Material materials with Elongación of 19.3 % | Predicted Value, A80 Transverse | |||||
20 °C | 13 % Show Material materials with Elongación of 13 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Estricción | 42.7 % Show Material materials with Estricción of 42.7 % | Predicted Value, Transverse | ||||
20 °C | 50 % Show Material materials with Estricción of 50 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Límite elástico | 318.7 MPa Show Material materials with Límite elástico of 318.7 MPa | Predicted Value, RP1 | ||||
326.9 MPa Show Material materials with Límite elástico of 326.9 MPa | Predicted Value, RP1 Transverse | |||||
347.3 MPa Show Material materials with Límite elástico of 347.3 MPa | Predicted Value, RP05 | |||||
517.9 MPa Show Material materials with Límite elástico of 517.9 MPa | Predicted Value, Transverse | |||||
573.8 MPa Show Material materials with Límite elástico of 573.8 MPa | Predicted Value, RP02 Transverse | |||||
745.8 MPa Show Material materials with Límite elástico of 745.8 MPa | Predicted Value, RP002 | |||||
866.7 MPa Show Material materials with Límite elástico of 866.7 MPa | Predicted Value, RP02 | |||||
20 °C | 750 MPa Show Material materials with Límite elástico of 750 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 800 MPa Show Material materials with Límite elástico of 800 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 850 MPa Show Material materials with Límite elástico of 850 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Módulo de cizallamiento | 80.3 GPa Show Material materials with Módulo de cizallamiento of 80.3 GPa | Predicted Value | ||||
Módulo elástico | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel | ||||
Resistencia a la tracción | 20 °C | 900 - 1300 MPa Show Material materials with Resistencia a la tracción of 900 - 1300 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | |
20 °C | 900 - 1200 MPa Show Material materials with Resistencia a la tracción of 900 - 1200 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 900 - 1100 MPa Show Material materials with Resistencia a la tracción of 900 - 1100 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 950 - 1300 MPa Show Material materials with Resistencia a la tracción of 950 - 1300 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 950 - 1200 MPa Show Material materials with Resistencia a la tracción of 950 - 1200 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 950 - 1100 MPa Show Material materials with Resistencia a la tracción of 950 - 1100 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 1050 - 1300 MPa Show Material materials with Resistencia a la tracción of 1050 - 1300 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 1050 - 1200 MPa Show Material materials with Resistencia a la tracción of 1050 - 1200 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 1050 - 1100 MPa Show Material materials with Resistencia a la tracción of 1050 - 1100 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Resistencia al cizallamiento | 532 MPa Show Material materials with Resistencia al cizallamiento of 532 MPa | Predicted Value |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 456.8 J/(kg·K) Show Material materials with Calor específico of 456.8 J/(kg·K) | Predicted Value |
Coeficiente de dilatación térmica | 12.21 1/K Show Material materials with Coeficiente de dilatación térmica of 12.21 1/K | Predicted Value |
Conductividad térmica | 36.54 W/(m·K) Show Material materials with Conductividad térmica of 36.54 W/(m·K) | Predicted Value |
Temperatura máx. de funcionamiento | 287.1 °C Show Material materials with Temperatura máx. de funcionamiento of 287.1 °C | Predicted Value, Long |
Eléctrico
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Boro | 0.0008 - 0.005 % Show Material materials with Boro of 0.0008 - 0.005 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
0.001 - 0.005 % Show Material materials with Boro of 0.001 - 0.005 % | quenched and tempered (+QT) | EN 10083-3, ISO 683-2 | Bar, Forging, Sheet, Strip, Flat | |
Carbono | 0.3 - 0.36 % Show Material materials with Carbono of 0.3 - 0.36 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Cobre | 0.4 % Show Material materials with Cobre of 0.4 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Cromo | 0.3 - 0.6 % Show Material materials with Cromo of 0.3 - 0.6 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Manganeso | 1.2 - 1.5 % Show Material materials with Manganeso of 1.2 - 1.5 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |