Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.7 g/cm³ Show Material materials with Densidad of 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Dureza Brinell | 20.0 °C | 230 [-] Show Material materials with Dureza Brinell of 230 [-] | |
Elongación | 20.0 °C | 40 % Show Material materials with Elongación of 40 % | |
Elongación A80 transversal | 20.0 °C | 40 % Show Material materials with Elongación A80 transversal of 40 % | |
Elongación transversal | 20.0 °C | 30 - 40 % Show Material materials with Elongación transversal of 30 - 40 % | |
Hardness, Brinell, trans | 20.0 °C | 230 [-] Show Material materials with Hardness, Brinell, trans of 230 [-] | |
Límite elástico Rp 0,2 | 20.0 °C | 210 MPa Show Material materials with Límite elástico Rp 0,2 of 210 MPa | |
100.0 °C | 185 MPa Show Material materials with Límite elástico Rp 0,2 of 185 MPa | ||
150.0 °C | 160 MPa Show Material materials with Límite elástico Rp 0,2 of 160 MPa | ||
200.0 °C | 145 MPa Show Material materials with Límite elástico Rp 0,2 of 145 MPa | ||
250.0 °C | 135 MPa Show Material materials with Límite elástico Rp 0,2 of 135 MPa | ||
300.0 °C | 125 MPa Show Material materials with Límite elástico Rp 0,2 of 125 MPa | ||
350.0 °C | 120 MPa Show Material materials with Límite elástico Rp 0,2 of 120 MPa | ||
400.0 °C | 115 MPa Show Material materials with Límite elástico Rp 0,2 of 115 MPa | ||
Límite elástico Rp 1,0 | 20.0 °C | 240 MPa Show Material materials with Límite elástico Rp 1,0 of 240 MPa | |
100.0 °C | 210 MPa Show Material materials with Límite elástico Rp 1,0 of 210 MPa | ||
150.0 °C | 190 MPa Show Material materials with Límite elástico Rp 1,0 of 190 MPa | ||
200.0 °C | 175 MPa Show Material materials with Límite elástico Rp 1,0 of 175 MPa | ||
250.0 °C | 165 MPa Show Material materials with Límite elástico Rp 1,0 of 165 MPa | ||
300.0 °C | 155 MPa Show Material materials with Límite elástico Rp 1,0 of 155 MPa | ||
350.0 °C | 150 MPa Show Material materials with Límite elástico Rp 1,0 of 150 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 210 - 220 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 210 - 220 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 240 - 260 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 240 - 260 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 20.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | |
100.0 °C | 194 GPa Show Material materials with Módulo elástico of 194 GPa | ||
200.0 °C | 186 GPa Show Material materials with Módulo elástico of 186 GPa | ||
300.0 °C | 179 GPa Show Material materials with Módulo elástico of 179 GPa | ||
400.0 °C | 172 GPa Show Material materials with Módulo elástico of 172 GPa | ||
500.0 °C | 165 GPa Show Material materials with Módulo elástico of 165 GPa | ||
Resistencia a la tracción | 20.0 °C | 530 - 730 MPa Show Material materials with Resistencia a la tracción of 530 - 730 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 530 - 730 MPa Show Material materials with Resistencia a la tracción transversal of 530 - 730 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | Typical for Austenitic Stainless Steel |
Coeficiente de dilatación térmica | 100.0 °C | 1.65E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 1/K | |
Conductividad térmica | 20.0 °C | 14 W/(m·K) Show Material materials with Conductividad térmica of 14 W/(m·K) | |
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Resistividad eléctrica | 23.0 °C | 8.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % |
Carbono | 0.015 % Show Material materials with Carbono of 0.015 % |
Cromo | 16.5 - 18.5 % Show Material materials with Cromo of 16.5 - 18.5 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 0.2 % Show Material materials with Molibdeno of 0.2 % |
Nitrógeno | 0.11 % Show Material materials with Nitrógeno of 0.11 % |
Níquel | 14 - 16 % Show Material materials with Níquel of 14 - 16 % |
Silicona | 3.7 - 4.5 % Show Material materials with Silicona of 3.7 - 4.5 % |