General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8 g/cm³ Show Material materials with Densidad of 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Dureza Brinell | 20.0 °C | 260 [-] Show Material materials with Dureza Brinell of 260 [-] | |
Elongación | 20.0 °C | 20 - 35 % Show Material materials with Elongación of 20 - 35 % | |
Elongación A80 transversal | 20.0 °C | 35 - 40 % Show Material materials with Elongación A80 transversal of 35 - 40 % | |
Elongación transversal | 20.0 °C | 30 - 40 % Show Material materials with Elongación transversal of 30 - 40 % | |
Límite elástico Rp 0,2 | 20.0 °C | 300 MPa Show Material materials with Límite elástico Rp 0,2 of 300 MPa | |
100.0 °C | 230 MPa Show Material materials with Límite elástico Rp 0,2 of 230 MPa | ||
150.0 °C | 205 MPa Show Material materials with Límite elástico Rp 0,2 of 205 MPa | ||
200.0 °C | 190 MPa Show Material materials with Límite elástico Rp 0,2 of 190 MPa | ||
250.0 °C | 180 MPa Show Material materials with Límite elástico Rp 0,2 of 180 MPa | ||
300.0 °C | 170 MPa Show Material materials with Límite elástico Rp 0,2 of 170 MPa | ||
350.0 °C | 165 MPa Show Material materials with Límite elástico Rp 0,2 of 165 MPa | ||
400.0 °C | 160 MPa Show Material materials with Límite elástico Rp 0,2 of 160 MPa | ||
450.0 °C | 153 MPa Show Material materials with Límite elástico Rp 0,2 of 153 MPa | ||
500.0 °C | 148 MPa Show Material materials with Límite elástico Rp 0,2 of 148 MPa | ||
Límite elástico Rp 1,0 | 20.0 °C | 340 MPa Show Material materials with Límite elástico Rp 1,0 of 340 MPa | |
100.0 °C | 270 MPa Show Material materials with Límite elástico Rp 1,0 of 270 MPa | ||
150.0 °C | 245 MPa Show Material materials with Límite elástico Rp 1,0 of 245 MPa | ||
200.0 °C | 225 MPa Show Material materials with Límite elástico Rp 1,0 of 225 MPa | ||
250.0 °C | 212 MPa Show Material materials with Límite elástico Rp 1,0 of 212 MPa | ||
300.0 °C | 200 MPa Show Material materials with Límite elástico Rp 1,0 of 200 MPa | ||
350.0 °C | 195 MPa Show Material materials with Límite elástico Rp 1,0 of 195 MPa | ||
400.0 °C | 190 MPa Show Material materials with Límite elástico Rp 1,0 of 190 MPa | ||
450.0 °C | 184 MPa Show Material materials with Límite elástico Rp 1,0 of 184 MPa | ||
500.0 °C | 180 MPa Show Material materials with Límite elástico Rp 1,0 of 180 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 300 - 320 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 300 - 320 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 340 - 350 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 340 - 350 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 20.0 °C | 195 GPa Show Material materials with Módulo elástico of 195 GPa | |
100.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | ||
200.0 °C | 182 GPa Show Material materials with Módulo elástico of 182 GPa | ||
300.0 °C | 174 GPa Show Material materials with Módulo elástico of 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Módulo elástico of 166 GPa | ||
500.0 °C | 158 GPa Show Material materials with Módulo elástico of 158 GPa | ||
Resistencia a la tracción | 20.0 °C | 650 - 1100 MPa Show Material materials with Resistencia a la tracción of 650 - 1100 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 650 - 850 MPa Show Material materials with Resistencia a la tracción transversal of 650 - 850 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.65E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 1/K | |
200.0 °C | 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K | ||
300.0 °C | 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 1/K | ||
400.0 °C | 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | ||
Conductividad térmica | 20.0 °C | 14 W/(m·K) Show Material materials with Conductividad térmica of 14 W/(m·K) | |
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | -60 - 400 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -60 - 400 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 8.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % |
Carbono | 0.02 % Show Material materials with Carbono of 0.02 % |
Cobre | 0.5 - 1 % Show Material materials with Cobre of 0.5 - 1 % |
Cromo | 19.5 - 20.5 % Show Material materials with Cromo of 19.5 - 20.5 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Molibdeno | 6 - 7 % Show Material materials with Molibdeno of 6 - 7 % |
Nitrógeno | 0.18 - 0.25 % Show Material materials with Nitrógeno of 0.18 - 0.25 % |
Níquel | 17.5 - 18.5 % Show Material materials with Níquel of 17.5 - 18.5 % |
Silicona | 0.7 % Show Material materials with Silicona of 0.7 % |